Figure 1:
Preparation of epoxy-coated and sand-coated glass fiber strands

Figure 2:
Types of glass fibers

Figure 3:
SEM micrographs of epoxy-coated and sand-coated glass fiber strands surrounded by cement mortar; (a) 10 [μm] scale, (b) 100 [μm] scale

Figure 4:
SEM micrographs of epoxy-coated glass fiber strands surrounded by cement mortar; (a) 20 [μm] scale, (b) 100 [μm] scale

Figure 5:
Compressive strength vs. percentage of glass fibers

Figure 6:
Comparison of compressive strength of concrete mixtures (x-axis represents the results of uncoated or epoxy-coated and sand-coated; y-axis represents the results of Epoxy-coated)

Figure 7:
Flexural strength vs. percentage of glass fibers

Figure 8:
Comparison of flexural strength of concrete mixtures (x-axis represents the results of uncoated or epoxy-coated and sand-coated; y-axis represents the results of epoxy-coated)

Figure 9:
Splitting strength vs. percentage of glass fibers

Figure 10:
Comparison of splitting strength of concrete mixtures (x-axis represents the results of uncoated or epoxy-coated and sand-coated; y-axis represents the results of Epoxy-coated)

Figure 11:
Flexural to compressive strength ratio

Figure 12:
Tensile strength of cement mortar briquettes

Figure 13:
Direct tensile strength test setup and failure modes of mortar briquette specimens
Table 1:
Chemical composition and specific gravity of ordinary Portland cement
| Component | Portland cement |
|---|---|
| SiO2 [%] | 19.8 |
| Al2O3 [%] | 4.13 |
| Fe2O3 [%] | 3.85 |
| CaO [%] | 61.87 |
| MgO [%] | 3.52 |
| SO3 [%] | 1.79 |
| Cl− [%] | 0.01 |
| LOI [%] | 2.35 |
| Specific Gravity [-] | 3.15 |
Table 2:
Physical properties of ordinary Portland cement
| Property | Value |
|---|---|
| Initial setting time [Minutes] | 125 |
| Final setting time [Minutes] | 300 |
| Blaine [m2/kg] | 300 |
| Expansion [%] | 0.04 |
| 3 days compressive strength [MPa] | 11 |
| 7 days compressive strength [MPa] | 18 |
| 28 days compressive strength [MPa] | 29 |
Table 3:
Properties of Glass fiber
Table 4:
Mixture proportions
| Mixtures* | Weight proportion (Cement: Fine agg.: Coarse agg.) | w/c | Cement [kg/m3] | Water [kg/m3] | Fine Aggregate [kg/m3] | Coarse Aggregate [kg/m3] | Super plasticizer [L/m3] |
|---|---|---|---|---|---|---|---|
| MC-0-U | 1:2.75:4 | 0.35 | 308 | 108 | 847 | 1232 | 2.04 |
| MGF-0.33-U | 1:2.75:4 | 0.35 | 308 | 108 | 847 | 1232 | 2.55 |
| MGF-0.66-U | 1:2.75:4 | 0.35 | 308 | 108 | 847 | 1232 | 3.05 |
| MGF-1.0-U | 1:2.75:4 | 0.35 | 308 | 108 | 847 | 1232 | 3.30 |
| MGF-0.33-C | 1:2.75:4 | 0.35 | 308 | 108 | 847 | 1232 | 2.55 |
| MGF-0.66-C | 1:2.75:4 | 0.35 | 308 | 108 | 847 | 1232 | 3.05 |
| MGF-1.0-C | 1:2.75:4 | 0.35 | 308 | 108 | 847 | 1232 | 3.30 |
| MGF-0.66-CS | 1:2.75:4 | 0.35 | 308 | 108 | 847 | 1232 | 3.05 |
| MGF-1.0-CS | 1:2.75:4 | 0.35 | 308 | 108 | 847 | 1232 | 3.30 |
Table 5:
Details of experimental test program and specimen quantities
| Test | Name of the standard test | Size / Details of Specimen | Number of specimens |
|---|---|---|---|
| Slump | ASTM C143 | Fresh concrete matrix | 1 per mixture (9 total) |
| Compressive strength | ASTM C39 | Concrete cylinder with a diameter of 6 in. [152 mm] and height of 12 in. [305 mm] | 3 per mixture (27 total) |
| Splitting strength | ASTM C496 | Concrete cylinder with a diameter of 6 in. [152 mm] and height of 12 in. [305 mm] | 3 per mixture (27 total) |
| Flexural strength | ASTM C78 | Concrete prism with dimensions of 4 in. × 4 in. × 20 in. [100 mm × 100 mm × 500 mm] | 3 per mixture (27 total) |
| The tensile strength of the epoxy-coated glass fiber strands | ASTM D7205-06 | Epoxy-coated glass fiber strand | 3 |
| Tensile strength (cement mortar) | ASTM C190 | Cement mortar briquette, 3 in. [75 mm] long, with a standardized necking cross-section of 1 in. × 1 in. [25 mm × 25 mm] | 3 |
| Tensile strength (cement mortar with 3 epoxy-coated glass fiber strands) * | ASTM C190 | Cement mortar briquette, 3 in. [75 mm] long, with a standardized necking cross-section of 1 in. × 1 in. [25 mm × 25 mm] | 3 |
| Tensile strength (cement mortar with 3 epoxy-coated and sand- coatedglass fiber strands) * | ASTM C190 | Cement mortar briquette, 3 in. [75 mm] long, with a standardized necking cross-section of 1 in. × 1 in. [25 mm × 25 mm] | 3 |
Table 6:
Concrete properties
| Mixtures* | Slump [mm] | Temp., [°C] |
|---|---|---|
| MC-0-U | 130 | 34.5 |
| MGF-0.33-U | 130 | 32.0 |
| MGF-0.66-U | 130 | 31.8 |
| MGF-1.0-U | 110 | 30.8 |
| MGF-0.33-C | 135 | 30.0 |
| MGF-0.66-C | 120 | 34.5 |
| MGF-1.0-C | 100 | 38.1 |
| MGF-0.66-CS | 115 | 30.5 |
| MGF-1.0-CS | 120 | 31.7 |
* Mixture designation: See Table 4
Table 7:
Mechanical properties of concrete [MPa]
| Mixtures* | Compressive strength (28 days) | Splitting strength (28 days) | Flexural strength (28 days) |
|---|---|---|---|
| MC-0-U | 37.4 | 2.3 | 2.8 |
| MGF-0.33-U | 48.8 | 3.1 | 3.9 |
| MGF-0.66-U | 51.6 | 3.4 | 4.1 |
| MGF-1.0-U | 51.6 | 4.1 | 4.6 |
| MGF-0.33-C | 49.7 | 3.0 | 4.5 |
| MGF-0.66-C | 46.2 | 2.9 | 5.0 |
| MGF-1.0-C | 47.6 | 3.7 | 5.0 |
| MGF-0.66-CS | 48.3 | 4.9 | 5.6 |
| MGF-1.0-CS | 49.8 | 5.5 | 5.7 |
* Mixture designation: See Table 4