Skip to main content
Have a personal or library account? Click to login
Experimental Investigation of Wall Thickness Effect on Cold Joints in a Scaled Diaphragm Wall Model Using Fiber-Reinforced Self-Compacting Concrete Cover

Experimental Investigation of Wall Thickness Effect on Cold Joints in a Scaled Diaphragm Wall Model Using Fiber-Reinforced Self-Compacting Concrete

Open Access
|Sep 2026
Read online

Figures & tables

Figure 1:

Leakage occurred at the joints between panels (Yang et al., 2024)

Table 1:

details of specimens

specimenWall thicknessNumber of cold jointsaspect ratio
[mm] thicknessdepth
T40-0400 160
T60-0600 140
T80-0800 130
T100-01000 124
T60-1601 140
T60-2602 140
T100-21002 124
Figure 2:

Specimens details (unite in m)

Figure 3:

Polypropylene Fiber

Table 2:

Mix proportions of Self-Compact Polypropylene Fiber-Reinforced Concrete (SCPPFRC)

Cement [kg/m3]Fly Ash [kg/m3]Sand [kg/m3]Gravel [kg/m3]Water [kg/m3]Admixture S.P. [kg/m3]Polypropylene Fiber P.P.F. [kg/m3]
35060a800725165b7c4.55d
a Fly Ash=17% of cement weight, b w/b =40%, c S.P./b=1.7% and d Polypropylene Fiber =0.5% of total volume
Mix strength grade, MPa at 28 days38.71
Figure 4:

V-funnel, slump flow and L-box tests of fresh concrete

Table 3:

Fresh properties result of SCC mix

MixProperties related to self-compact ability
Slump flow [mm]T50cm flow time [Sec]V-funnel time [Sec]L-box (H2/H1)
SCCa680480.98
SCPFRCb6156210.76
Typical range of values (EFNARC, 2005)650-8002–56–120.8–1.0

a. SCC: Self - Compacting Concrete

b. SC-PFRC: Self-compact Polypropylene Fiber-Reinforced Concrete

Figure 5:

Shows the testing process of the concrete material parameters.

Table 4:

Mechanical properties of concrete

Compressive Strength [MPa]Splitting tensile strength [MPa]Flexural strength [MPa]Elastic Modulus [GPa]
38.714.864.6233
Table 5:

Mechanical properties of steel reinforcements

Nominal diameter [mm]Actual Diameter [mm]Yield Stress [MPa]Ultimate Stress [MPa]Elastic Modulus [GPa]
65.9430560200
Figure 6:

Schematic diagram of the specimen monitoring system (unit: m)

Figure 7:

Experimental Loading Setup System

Figure 8:

Load-midspan deflection curves of specimens with different thicknesses

Table 6:

Characteristic loads, midspan deflections of specimens with different thickness

specimenStiffness RatioPyieldδyieldPultimateδultimatePcr
EI/γw*h4[kN][mm][kN][mm][kN]
T40-04341.705. 60249.251.72
T60-01465(↑238%)*3.80(↑124%)*5.40 (↓4%)*6.07(↑204%)*43.55(↓12%)*3.86(↑124%)*
T80-03472(↑700%)*5.40(↑218%)*2.80 (↓50%)*7.8(↑290%)*22.80(↓54%)*5.50(↑220%)*
T100-06782(↑1463%)*8.20(↑382%)*2.38(↓58%)*9.40(↑370%)*13.85(↓72%)*8.28(↑381%)*

Note: Pyield, δyield is the yield load and yield midspan deflections; Pultimate, δultimate is the ultimate load and ultimate midspan deflections; Pcr is the cracking load noted from experimental testing.

* Compared with specimens with 40mm thickness.

Figure 9:

Relations of Load and Midspan deflection with different thicknesses of specimens

Figure 10:

Load- midspan deflection curves of specimens with cold joints

Table 7:

Characteristic loads, midspan deflections of specimens with cold joints

specimenStiffness RatioPyieldδyieldPultimateδultimatePcr
EI/γw*h4[kN][mm][kN][mm][kN]
T60-114653.1(↓18%)*5.0(↓7%)*5.9(↓3%) *48.00(↑10%)*3.32(↓14%)*
T60-214652.65 (↓30%)*4.9 (↓9%)*5.14) ↓15%)*52.92 (↑22%)*2.78(↓28%)*
T100-267827.4 (↓10%)*3.0 (↑26%)*8.46(↓10%)*16.62(↑20%) *7.46(↓10%)*

Note: Pyield, δyield is the yield load and yield midspan deflections; Pultimate, δultimate is the ultimate load and ultimate midspan deflections; Pcr is the cracking load,

* Compared with specimen have same thickness but without cold joint.

Figure 11:

Effect Number of cold joints on load of specimens

Figure 12:

Effect Number of cold joints on midspan deflection of specimens

Figure 13:

Effect Number of cold joints on variation of load and midspan deflection of specimens

Figure 14:

Failure Mode

Figure 15:

Relationship between length of the segments (L) to its thickness (T) and depth of excavation (H) relative to thickness (T)

Figure 16:

Relationship of segment length-to-thickness ratio and the maximum lateral displacement δhmax of the diaphragm wall

Figure 17:

Relationship of Maximum Wall Deflection and Wall’s System Stiffness (Mana & Clough, 1981)

Table 8:

Ductility index of tested specimens

specimenδyieldδultimateDuctility
[mm][mm] μ=δmaxδyield
T40-05. 6049.258.80
T60-05.4043.558.10
T80-02.8022.808.00
T100-02.3813.855.82
T60-15.0048.009.00
T60-24.9052.9210.80
T100-23.0016.625.50
Figure 18:

Ductility of specimens with different thicknesses

Figure 19:

Ductility of specimens with number of cold joints

Figure 20:

Definition of yielding load (Feng et al., 2017)

Figure 21:

Relation the load with distance from the line

Table 9:

Definition of yielding load by Farthest Point Method

specimenWall thicknessNumber of cold jointsdmaxPyieldδyieldPyield by Tangent Intersection Method
[mm]------[mm][kN][mm][kN]
T40-04001.481.705.251.70
T60-06003.033.785.223.80
T80-08004.235.412.755.40
T100-010005.448.032.308.20
T60-16012.653.224.753.10
T60-26022.222.725.042.65
T100-210025.277.382.887.40
DOI: https://doi.org/10.2478/cee-2026-0067 | Journal eISSN: 2199-6512 (formerly 1336-5835) | Journal ISSN: 1336-5835
Language: English
Page range: 1064 - 1084
Submitted on: Oct 21, 2025
Accepted on: Nov 23, 2025
Published on: Sep 25, 2026
Published by: University of Žilina
In partnership with: Paradigm Publishing Services
Publication frequency: 4 issues per year

© 2026 Rana F. Yousef, Haitham H. Muteb, Ahmed Al-Janabi, published by University of Žilina
This work is licensed under the Creative Commons Attribution 4.0 License.