Table 1
Binder systems, activation routes and main findings of previous printable alkali-activated and cementless materials compared with the present study.
| Study | Binder (mass%) | Activation | Specimens | Main findings |
|---|---|---|---|---|
| Panda et al. [21] | Fly ash with up to 10% GGBS or silica fume | Alkaline activator solution; ambient curing | Printed and cast | GGBS raised early strength; silica fume improved viscosity recovery |
| Kondepudi and Subramaniam [22] | Fly ash–slag with micro-silica and clay | Alkaline solution with CMC viscosity modifier | Printed | Buildability linked to thixotropic build-up; particle size distribution controlled phase separation |
| Kondepudi et al. [28] | Fly ash–slag paste, varying aggregate content | Alkaline activator; nano-clay | Printed | Static yield stress set by solid surface area relative to paste volume; paste demand set by aggregate packing |
| Marczyk et al. [24] | Fly ash or metakaolin geopolymer + 5% cement; cement + 5% geopolymer | Alkaline activator | Printed | Rheology dependent on liquid-to-solid ratio; cement-based hybrid allowed detailed printing |
| Fiala et al. [4] | 10% GGBS–40% ultra-fine FA–50% FA | None (2 M NaOH variant also tested) | Printed, w/b 0.25 | About 1 MPa without activator; >10 MPa with 2 M NaOH |
| Lin et al. [25] | 50% Ultra-fine FA–50% CFA | None | Printed | 28-day strength 9 MPa; thermal conductivity 0.21 W/(m·K) |
| Lin et al. [16] | 70% GGBS–25% CFA–5% FGD gypsum | None (CFA, gypsum) | Cast paste; pervious concrete | Paste strength up to 79% of cement control; pervious concrete 12 MPa |
| Chen et al. [27] | 60% GGBS–30/35% CFA–10/5% FA | None (CFA) | Printed (print–rest–print) | 56-day axial and lateral compressive strength; thermal-conduction performance |
| Present study | 60% GGBS–30/35% CFA–10/5% FA; s/b 1.00–1.75; FM 1.2 and 1.7 | None (CFA) | Printed, 16 mixtures | Buildability, anisotropy, and flexure related to V p and FM; factorial separation of s/b, FM, and binder |

Figure 1
SEM photos of raw materials (3,000×). (a) GGBS, (b) FA, (c) CFA.
Table 2
Chemical compositions of raw materials.
| GGBS | CFA | Fly ash | |
|---|---|---|---|
| Loss of ignition, % | 0.10 | – | 1.00 |
| SiO2, % | 24.35 | 25.75 | 45.76 |
| Al2O3, % | 20.92 | 30.11 | 32.76 |
| CaO, % | 44.49 | 24.08 | 6.04 |
| Fe2O3, % | 0.70 | 4.38 | 8.80 |
| MgO, % | 5.64 | 1.80 | 1.38 |
| SO3, % | 2.05 | 9.87 | 0.80 |
| Na2O, % | 0.22 | 1.46 | 0.95 |
| K2O, % | 0.33 | 0.56 | 1.35 |
| TiO2, % | 1.00 | 0.94 | 1.26 |
| MnO, % | 0.22 | 0.06 | 0.08 |
Note: “–” is not measured items.

Figure 2
XRD patterns of the raw materials (GGBS, FA, and CFA).

Figure 3
Particle size distributions of the binders: (a) differential volume distribution; (b) cumulative passing curves.

Figure 4
Blockages in the print nozzle.
Table 3
Parameters for mix design.
| Mix no. | GGBS (%) | CFA (%) | FA (%) | s/b (FM 1.2) | s/b (FM 1.7) | w/b |
|---|---|---|---|---|---|---|
| A1 | 60 | 30 | 10 | 1.00 | – | 0.50 |
| A2 | 60 | 30 | 10 | 1.25 | – | 0.54 |
| A3 | 60 | 30 | 10 | 1.50 | – | 0.55 |
| A4 | 60 | 30 | 10 | 1.75 | – | 0.55 |
| B1 | 60 | 30 | 10 | – | 1.00 | 0.48 |
| B2 | 60 | 30 | 10 | – | 1.25 | 0.53 |
| B3 | 60 | 30 | 10 | – | 1.50 | 0.55 |
| B4 | 60 | 30 | 10 | – | 1.75 | 0.55 |
| C1 | 60 | 35 | 5 | 1.00 | – | 0.53 |
| C2 | 60 | 35 | 5 | 1.25 | – | 0.53 |
| C3 | 60 | 35 | 5 | 1.50 | – | 0.53 |
| C4 | 60 | 35 | 5 | 1.75 | – | 0.53 |
| D1 | 60 | 35 | 5 | – | 1.00 | 0.49 |
| D2 | 60 | 35 | 5 | – | 1.25 | 0.52 |
| D3 | 60 | 35 | 5 | – | 1.50 | 0.55 |
| D4 | 60 | 35 | 5 | – | 1.75 | 0.55 |

Figure 5
Mortar-type 3D printer.

Figure 6
Appearance of the printed specimens. (a) Buildability specimen, (b) printed compressive specimen, (c) printed flexural specimen.

Figure 7
Appearance for mini slump measurement.

Figure 8
Simulated appearance of printed specimen.
Table 4
Printability of cementless mortar.
| Mix no. | s/b | FM | Printability for stage I | Printability for stage II | ||||||
|---|---|---|---|---|---|---|---|---|---|---|
| w/b | Flowability (mm) | Mini slump (cm) | w/b | SP by binder (%) | Flowability (mm) | Mini slump (cm) | Printed layers | |||
| A1 | 1.00 | 1.2 | 0.55 | 150 | 11.0 | 0.50 | — | 150 | 7.5 | 11 |
| A2 | 1.25 | 150 | 10.0 | 0.54 | — | 150 | 8.5 | 11 | ||
| A3 | 1.50 | 150 | 6.5 | 0.55 | — | 150 | 6.5 | 11 | ||
| A4 | 1.75 | 122 | 4.5 | 0.55 | 0.05 | 150 | 6.7 | 15 | ||
| B1 | 1.00 | 1.7 | 150 | 12.2 | 0.48 | — | 138 | 7.8 | 11 | |
| B2 | 1.25 | 150 | 10.8 | 0.53 | — | 150 | 9.0 | 6 | ||
| B3 | 1.50 | 150 | 7.5 | 0.55 | — | 150 | 7.5 | 11 | ||
| B4 | 1.75 | 130 | 5.5 | 0.55 | 0.05 | 131 | 6.0 | 19 | ||
| C1 | 1.00 | 1.2 | 150 | 10.0 | 0.53 | — | 150 | 9.0 | 6 | |
| C2 | 1.25 | 150 | 10.0 | 0.53 | — | 150 | 7.2 | 10 | ||
| C3 | 1.50 | 132 | 6.0 | 0.53 | — | 132 | 6.0 | 10 | ||
| C4 | 1.75 | 114 | 4.2 | 0.53 | 0.05 | 150 | 7.0 | 12 | ||
| D1 | 1.00 | 1.7 | 150 | 12.2 | 0.49 | — | 135 | 7.2 | 12 | |
| D2 | 1.25 | 150 | 10.0 | 0.52 | — | 138 | 8.2 | 11 | ||
| D3 | 1.50 | 150 | 8.4 | 0.55 | — | 150 | 8.4 | 15 | ||
| D4 | 1.75 | 129 | 5.0 | 0.55 | 0.10 | 150 | 7.5 | 13 | ||

Figure 9
Initial and final setting times of the mixtures.

Figure 10
Predictors of stacking capacity: (a) printed layers versus mini-slump; (b) printed layers versus initial setting time; (c) printed layers versus sand-to-binder ratio.
Table 5
Derived skeleton and performance parameters of the sixteen printed mixtures.
| Mix no. | s/b | FM | w/b | V p | f ax (MPa) | f lat (MPa) | AI | f f (MPa) | k |
|---|---|---|---|---|---|---|---|---|---|
| A1 | 1.00 | 1.2 | 0.50 | 0.688 | 28.65 (0.47) | 17.74 (0.08) | 0.619 | 3.53 (0.22) | 0.659 |
| A2 | 1.25 | 1.2 | 0.54 | 0.649 | 27.27 (0.65) | 13.91 (0.17) | 0.510 | 4.33 (0.20) | 0.829 |
| A3 | 1.50 | 1.2 | 0.55 | 0.609 | 25.12 (0.55) | 14.61 (0.37) | 0.582 | 4.70 (0.79) | 0.938 |
| A4 | 1.75 | 1.2 | 0.55 | 0.571 | 22.84 (0.87) | 14.75 (0.11) | 0.646 | 4.73 (0.93) | 0.990 |
| B1 | 1.00 | 1.7 | 0.48 | 0.683 | 28.01 (0.94) | 16.44 (0.48) | 0.587 | 4.89 (0.21) | 0.924 |
| B2 | 1.25 | 1.7 | 0.53 | 0.646 | 23.85 (0.90) | 18.43 (0.24) | 0.773 | 4.05 (0.77) | 0.829 |
| B3 | 1.50 | 1.7 | 0.55 | 0.609 | 21.01 (0.81) | 17.09 (0.06) | 0.813 | 5.21 (0.45) | 1.137 |
| B4 | 1.75 | 1.7 | 0.55 | 0.571 | 24.85 (0.53) | 15.64 (0.37) | 0.629 | 6.09 (0.65) | 1.222 |
| C1 | 1.00 | 1.2 | 0.53 | 0.694 | 26.97 (0.97) | 19.46 (0.06) | 0.722 | 4.13 (0.46) | 0.795 |
| C2 | 1.25 | 1.2 | 0.53 | 0.645 | 26.44 (0.51) | 17.71 (0.54) | 0.670 | 4.76 (0.14) | 0.926 |
| C3 | 1.50 | 1.2 | 0.53 | 0.602 | 20.65 (0.31) | 13.29 (0.10) | 0.644 | 3.49 (0.16) | 0.768 |
| C4 | 1.75 | 1.2 | 0.53 | 0.565 | 23.86 (0.06) | 15.48 (0.12) | 0.649 | 3.95 (0.33) | 0.809 |
| D1 | 1.00 | 1.7 | 0.49 | 0.684 | 26.33 (0.39) | 20.10 (0.14) | 0.763 | 5.99 (0.90) | 1.167 |
| D2 | 1.25 | 1.7 | 0.52 | 0.642 | 25.53 (0.19) | 14.70 (0.44) | 0.576 | 4.77 (0.36) | 0.944 |
| D3 | 1.50 | 1.7 | 0.55 | 0.607 | 23.73 (0.12) | 16.10 (0.15) | 0.678 | 6.05 (0.48) | 1.242 |
| D4 | 1.75 | 1.7 | 0.55 | 0.570 | 21.29 (0.25) | 16.07 (0.07) | 0.755 | 5.67 (0.08) | 1.229 |
| Mean | — | — | — | 0.627 | 24.77 | 16.34 | 0.663 | 4.77 | 0.963 |
Note: All values are at 56 days; strengths are means of three specimens, with standard deviations in parentheses.

Figure 11
Development of the compressive strength of the printed specimens from 7 to 56 days: (a) axial (X-direction); (b) lateral (Y-direction); (c) anisotropy index (error bars: ± one standard deviation, n = 3).

Figure 12
Relationship between the 56-day axial compressive strength and the paste volume fraction, with pooled and series-specific linear fits (shaded band: 95% confidence interval of the pooled fit).

Figure 13
Directional strength of the printed mortar at 56 days: (a) axial and lateral strength of the printed specimens versus the strength of mould-cast cubes; (b) lateral versus axial compressive strength; (c) anisotropy index versus axial compressive strength.

Figure 14
Flexural strength of the mixtures at 56 days (error bars: ± one standard deviation, n = 3).

Figure 15
Flexural behaviour at 56 days: (a) effect of aggregate fineness modulus; (b) flexural strength versus the square root of the axial compressive strength, with the mean k for each sand grading and the code-based and geopolymer reference values.

Figure 16
SEM photos for A1 and A4 specimens (phase labels indicate tentative assignments based on morphology and EDS). (a) A1 specimen (×3,000), (b) A1 specimen (×5,000), (c) A4 specimen (×3,000), (d) A4 specimen (×10,000), (e) unreacted FA in A4 (×5,000).
Table 6
EDS results for A1 and A4 specimens (wt.%).
| Element | Content (wt.%) | ||
|---|---|---|---|
| A1 from Figure 16a | A1 from Figure 16b | A4 from Figure 16c | |
| Ca | 32.45 | 21.82 | 42.87 |
| Si | 7.24 | 10.30 | 4.75 |
| Al | 3.06 | 4.66 | — |
| S | 1.43 | 3.45 | — |
| O | 55.82 | 59.77 | 52.38 |

Figure 17
XRD patterns of the hardened paste fraction of mixtures A1, B1, C1 and D1, compared with the raw CFA.
Table 7
Three-way ANOVA (main effects) of the design factors on the measured and derived responses.
| Response | s/b: p (ηp 2) | FM: p (η p 2) | Binder: p (η p 2) | Model R 2 |
|---|---|---|---|---|
| Printed layers | 0.073 (0.49) | 0.287 (0.11) | 0.587 (0.03) | 0.52 |
| Initial setting time | 0.034 (0.56) | 0.004 (0.59) | 0.315 (0.10) | 0.74 |
| f ax | 0.004 (0.72) | 0.276 (0.12) | 0.302 (0.11) | 0.74 |
| f lat | 0.079 (0.48) | 0.277 (0.12) | 0.532 (0.04) | 0.52 |
| AI | 0.866 (0.07) | 0.155 (0.19) | 0.413 (0.07) | 0.28 |
| f f | 0.601 (0.16) | 0.008 (0.53) | 0.650 (0.02) | 0.57 |
| k | 0.150 (0.40) | 0.003 (0.61) | 0.495 (0.05) | 0.70 |
Note: Main-effects ANOVA on the 16 mixture means; η p 2, partial eta-squared; bold values, p < 0.05.