Skip to main content
Have a personal or library account? Click to login
Paste volume fraction and aggregate fineness as design parameters for 3D-printed self-activated cementless mortars: buildability, compressive anisotropy, and flexural response Cover

Paste volume fraction and aggregate fineness as design parameters for 3D-printed self-activated cementless mortars: buildability, compressive anisotropy, and flexural response

Open Access
|Nov 2026
Read online

Full article

1. Introduction

The transition toward sustainable construction was necessitated by the urgent need to reduce the substantial carbon footprint and energy consumption of ordinary Portland cement (OPC) [1,2]. Consequently, the development of alternative binders became a critical focus [3]. Cementless alkali-activated materials (AAMs), or geopolymers, emerged as viable pathways toward net-zero emissions [4,5]. These systems utilized industrial by-products, including ground granulated blast-furnace slag (GGBS), fly ash (FA), and co-fired fly ash (CFA) [4,6], to form a binding matrix via geopolymerization [7]. Substituting OPC with these materials significantly reduced carbon intensity [8] and promoted a circular economy [9,10].

However, conventional AAMs required energy- and carbon-intensive alkaline activators [11–13], complicating their environmental benefits. To address this, research advanced toward self-hardening materials from high-alkali waste [4,14] and optimized blended AAM systems [15]. This study followed the first route. It used a ternary binder of GGBS, FA, and CFA without any external alkaline activator; the term self-activated was used here for a binder in which the alkalinity and sulfate needed to dissolve GGBS were supplied internally by the free lime and anhydrite of CFA [16,17], as distinct from alkali-activated materials prepared with hydroxide or silicate solutions.

Integrating these sustainable binders with 3D concrete printing (3DCP) offered reduced waste, lower costs and enhanced design freedom [6,18,19], provided printability, strength, and durability were adequately balanced [20]. Researchers developed printable alkali-activated systems mainly from fly ash–slag blends activated with alkaline solutions. Panda et al. found that up to 10% GGBS in a fly ash geopolymer raised early strength, whereas silica fume governed the recovery of viscosity [21]; Kondepudi and Subramaniam achieved buildability in activated fly ash–slag mixtures only after enhancing thixotropic build-up with clay and a cellulose viscosity modifier [22]; and Bong et al. formulated a one-part, ambient-cured just-add-water geopolymer to avoid handling corrosive activator solutions [23]. Researchers also printed hybrid fly ash and metakaolin geopolymers with small cement additions, with rheology depending strongly on the liquid-to-solid ratio [24]. Activator-free cementless binders received far less attention. A ternary blend of 10% GGBS, 40% ultra-fine fly ash and 50% fly ash was printable but reached only about 1 MPa without an activator [4], and printed binary ultra-fine fly ash–CFA specimens reached 9 MPa at 28 days [25]. GGBS–CFA systems, in which CFA supplied free lime and anhydrite, developed considerably higher strength in cast form [16,26], and the present authors subsequently printed GGBS–CFA–FA mortars [27]. Table 1 compares the binder proportions, activation route, and main findings of these studies with the present work.

Table 1

Binder systems, activation routes and main findings of previous printable alkali-activated and cementless materials compared with the present study.

StudyBinder (mass%)ActivationSpecimensMain findings
Panda et al. [21]Fly ash with up to 10% GGBS or silica fumeAlkaline activator solution; ambient curingPrinted and castGGBS raised early strength; silica fume improved viscosity recovery
Kondepudi and Subramaniam [22]Fly ash–slag with micro-silica and clayAlkaline solution with CMC viscosity modifierPrintedBuildability linked to thixotropic build-up; particle size distribution controlled phase separation
Kondepudi et al. [28]Fly ash–slag paste, varying aggregate contentAlkaline activator; nano-clayPrintedStatic yield stress set by solid surface area relative to paste volume; paste demand set by aggregate packing
Marczyk et al. [24]Fly ash or metakaolin geopolymer + 5% cement; cement + 5% geopolymerAlkaline activatorPrintedRheology dependent on liquid-to-solid ratio; cement-based hybrid allowed detailed printing
Fiala et al. [4]10% GGBS–40% ultra-fine FA–50% FANone (2 M NaOH variant also tested)Printed, w/b 0.25About 1 MPa without activator; >10 MPa with 2 M NaOH
Lin et al. [25]50% Ultra-fine FA–50% CFANonePrinted28-day strength 9 MPa; thermal conductivity 0.21 W/(m·K)
Lin et al. [16]70% GGBS–25% CFA–5% FGD gypsumNone (CFA, gypsum)Cast paste; pervious concretePaste strength up to 79% of cement control; pervious concrete 12 MPa
Chen et al. [27]60% GGBS–30/35% CFA–10/5% FANone (CFA)Printed (print–rest–print)56-day axial and lateral compressive strength; thermal-conduction performance
Present study60% GGBS–30/35% CFA–10/5% FA; s/b 1.00–1.75; FM 1.2 and 1.7None (CFA)Printed, 16 mixturesBuildability, anisotropy, and flexure related to V p and FM; factorial separation of s/b, FM, and binder

In printable mortars, the fine aggregate acted as the primary rheological modifier [29]. Increasing the s/b raised interparticle friction, yield stress and pumping pressure [30,31]. Although a higher s/b reduced shrinkage and carbon footprint, excessive ratios caused extrusion problems and clogging [18,32]; fine aggregate contents of 600–800 kg/m3 were recommended [33]. Grading also mattered: optimizing sand gradation with the Fuller–Thompson curve and a packing-based viscosity model improved both rheology and buildability of printed mortar [34], and FM was linked to rheology and interparticle voids [35,36]. For alkali-activated fly ash–slag mortars, Kondepudi et al. showed that static yield stress depended on the solids surface area relative to paste volume. Paste content had to exceed the demand set by aggregate packing [28]. These findings pointed to the paste volume, rather than s/b or w/b separately, as the quantity linking aggregate content to fresh and hardened behavior. Buildability itself was usually framed as a rheological problem, in which the static yield stress and its rate of structural build-up had to keep pace with the stress imposed by the overlying layers [37]; in practice, these quantities were often approximated by slump-type and flow tests [38,39], whose ability to rank the stacking capacity of mixtures with different aggregate skeletons had seldom been examined.

In the hardened state, layer-wise deposition produced interlayer interfaces that acted as planes of weakness, so that compressive and flexural strengths depended on the loading direction [40–42]. Process variables largely controlled interlayer strength, notably the time interval between layers and the substrate surface moisture [43,44], and interface properties governed the mechanical performance of printed elements [45]. For cementless and alkali-activated printed mortars, it remained unclear whether mix-design variables that increased bulk strength also increased interlayer capacity, and whether flexural strength scaled with compressive strength as code relationships for conventional concrete assumed [46,47].

Although s/b [32], FM [35,36], and binder rheology [6,22,28] were each studied, researchers generally treated these variables as independent design levers and rarely asked which was associated with stacking capacity once the fresh state was held within one workability window. Moreover, data for activator-free GGBS–CFA systems were limited to cast specimens or to a small number of printable mixtures (Table 1). This study aimed to determine whether V p and FM could serve as practical design parameters for a self-activated GGBS–CFA–FA cementless mortar (CM) printed under fixed process conditions. The specific objectives were (i) to test, against measured data, three explanations commonly offered for buildability, namely shape retention, setting kinetics, and the granular skeleton; (ii) to relate the 56-day axial compressive strength to V p and to quantify the anisotropy between axial and lateral strength; (iii) to evaluate the flexural response and its relation to compressive strength; and (iv) to separate the effects of s/b, FM, and binder composition by regression and factorial analysis of variance.

A companion letter by the present authors [27] introduced a print–rest–print strategy for this mortar, exploiting its long setting time to reach 30 layers without accelerators, and reported the thermal conductivity, 56-day axial and lateral compressive strengths, and the microstructure of a single mixture (B4). It did not examine continuous-printing stacking capacity, strength development, comparison with mould-cast specimens, flexural response or the effects of design factors. Only the 56-day compressive strengths were shared with [27] and were used here solely to derive V p, AI and k; all other data, namely the fresh properties and layer counts, setting times, 7- and 28-day compressive strengths, the strengths of mould-cast reference cubes, flexural strengths, scanning electron microscopy with energy-dispersive X-ray spectroscopy (SEM–EDS) observations and X-ray diffraction (XRD) of the hardened pastes, were reported here for the first time. The contribution of the present work therefore lay in fully characterizing the 16 printed mixtures mechanically and separating the effects of skeleton parameters on buildability, anisotropy, and flexural strength.

2. Materials and methods

2.1. Materials

Three industrial by-products, GGBS, CFA, and FA, were used as the binder (Figure 1). Their specific gravities were 2.88, 2.71, and 2.20 and their fineness values 6,010, 4,560, and 5,220 cm2/g, respectively; their chemical compositions are given in Table 2. GGBS was a calcium aluminosilicate (CaO 44.49%, SiO2 24.35%, Al2O3 20.92%), and FA was a low-calcium siliceous ash (CaO 6.04%; SiO2 + Al2O3 + Fe2O3 = 87.32%). CFA, produced in a circulating fluidized bed (CFB) boiler with in-bed limestone desulfurization, combined an intermediate CaO content (24.08%) with a high SO3 content (9.87%). In such ashes, the limestone is calcined at a furnace temperature too low for the lime to react with the ash, so much of the CaO remains as free lime (f-CaO) and the captured sulfur as anhydrite (CaSO4) [17,48,49]; these supply the alkalinity and sulfate that activate GGBS. The f-CaO content was not determined chemically, but the XRD pattern of the CFA (Figure 2) showed anhydrite, calcite, portlandite, and quartz with a weak lime reflection at about 37.4° 2θ, indicating that part of the free lime remained unhydrated and the remainder had hydrated or carbonated during storage. GGBS was largely amorphous, with a broad hump centred at about 31° 2θ and a trace of calcite, whereas FA contained quartz, mullite, and hematite on a glassy hump at about 15°–35° 2θ. Figure 3 shows the particle size distributions of the binders; the median particle sizes (d50) were 7.8 μm for GGBS, 11.1 μm for FA, and 25.9 μm for CFA (Figure 3b). Lanyang River sand with fineness moduli of 1.2, 1.7, and 2.6 was used as the fine aggregate; its saturated-surface-dry (SSD) specific gravity was 2.55, and its water absorption was 1.83%. The sand was batched oven-dry without correcting the mixing water; the reported w/b values are nominal. The water it could absorb corresponds to at most 0.032 of w/b and was implicitly accounted for by the iso-workability adjustment. A powdered polycarboxylate-ether superplasticizer (SP; 800 F, Triaxis, Taipei, Taiwan; active content ≥ 90%) was used where required and was added to the dry materials before mixing.

Figure 1

SEM photos of raw materials (3,000×). (a) GGBS, (b) FA, (c) CFA.

Table 2

Chemical compositions of raw materials.

GGBSCFAFly ash
Loss of ignition, %0.10 – 1.00
SiO2, %24.3525.7545.76
Al2O3, %20.9230.1132.76
CaO, %44.4924.086.04
Fe2O3, %0.704.388.80
MgO, %5.641.801.38
SO3, %2.059.870.80
Na2O, %0.221.460.95
K2O, %0.330.561.35
TiO2, %1.000.941.26
MnO, %0.220.060.08

Note: “–” is not measured items.

Figure 2

XRD patterns of the raw materials (GGBS, FA, and CFA).

Figure 3

Particle size distributions of the binders: (a) differential volume distribution; (b) cumulative passing curves.

2.2. Mix design and specimens

Building upon previous research [50], CM mixtures were designed with binders of either 60% GGBS–35% CFA–5% FA or 60% GGBS–30% CFA–10% FA. Fine aggregates were incorporated at s/b = 1.75, 1.50, 1.25, 1.00, and 0.75; however, frequent nozzle blockages (Figure 4) occurred at s/b = 0.75 and with FM = 2.6, and these settings were therefore excluded. The resulting mixtures are summarised in Table 3 using fine (FM = 1.2) and coarse (FM = 1.7) sand. An iso-workability method was adopted in which w/b was adjusted iteratively, with SP added where w/b alone was insufficient (0.05% by mass of binder for A4, B4, and C4 and 0.10% for D4), to achieve a target mini-slump of 5.0–10.0 cm; Table 3 gives the final (Stage II) w/b values. The w/b and SP were therefore dependent variables, whereas s/b (four levels), FM (two levels) and binder composition (two levels) were the independent design factors of a full 4 × 2 × 2 factorial.

Figure 4

Blockages in the print nozzle.

Table 3

Parameters for mix design.

Mix no.GGBS (%)CFA (%)FA (%)s/b (FM 1.2)s/b (FM 1.7)w/b
A16030101.00 – 0.50
A26030101.25 – 0.54
A36030101.50 – 0.55
A46030101.75 – 0.55
B1603010 – 1.000.48
B2603010 – 1.250.53
B3603010 – 1.500.55
B4603010 – 1.750.55
C1603551.00 – 0.53
C2603551.25 – 0.53
C3603551.50 – 0.53
C4603551.75 – 0.53
D160355 – 1.000.49
D260355 – 1.250.52
D360355 – 1.500.55
D460355 – 1.750.55

2.3. Testing methods and specimens

2.3.1. 3D printing and specimen preparation

A UM2205 mortar printer (Figure 5) was utilized for fabrication. CM was prepared using a three-stage mixing procedure: 10 min of dry-mixing, 10 min of low-speed mixing (139 RPM) with water, and 5 min of high-speed mixing (285 RPM) with manual stirring. Printing was executed at 30 mm/s using a 15-mm nozzle. Three types of specimens were printed:

  1. Buildability specimens: 30-layer hollow cylinders (15 cm diameter, 0.8 cm layer thickness) (Figure 6a).

  2. Compressive strength specimens: 7-layer prisms sectioned into 5-cm cubes (Figure 6b).

  3. Flexural strength specimens: 6-layer structures measuring 4 cm × 4 cm × 16 cm (Figure 6c).

Figure 5

Mortar-type 3D printer.

Figure 6

Appearance of the printed specimens. (a) Buildability specimen, (b) printed compressive specimen, (c) printed flexural specimen.

Each 8 mm layer was deposited using a 15 mm circular nozzle (layer height-to-nozzle diameter ratio 0.53), flattening and pressing the filament onto the underlying layer and promoting interlayer contact [37,43]. The nozzle, layer height, printing speed, and toolpath, and thus the interlayer time interval, were identical for all mixtures, so the interface deposition conditions were common across the entire experimental matrix.

All specimens were air-cured. After printing (and demoulding where applicable), they were stored in laboratory air at room temperature, without sealing, water immersion, or heat curing, until the test ages of 7, 28, and 56 days; the laboratory temperature was 23 ± 2°C and the relative humidity was 65 ± 5%.

2.3.2. Printability and mechanical properties tests

Flow tests and setting times were determined in accordance with ASTM C1437 and ASTM C191, respectively. Target workability was evaluated using a modified half-scale mini-slump cone (Figure 7). Buildability was assessed as the number of layers printed continuously, without any rest interval, before collapse or excessive deformation of the cylinders (Figure 6a), unlike the print–rest–print strategy of [27].

Figure 7

Appearance for mini slump measurement.

Compressive strength was tested on 50 mm cubes at 7, 28, and 56 days (ASTM C109) in both the vertical (X-axis, axial) and lateral (Y-axis) directions to account for print-induced anisotropy (Figure 8). As a non-printed reference, 50 mm cubes were cast in steel moulds from the same batches, demoulded after 24 h, air-cured identically, and tested at 28 and 56 days. Flexural strength was determined at 56 days on 40 mm × 40 mm × 160 mm printed prisms in three-point bending (ASTM C348), with the load applied in the X-direction only. Each result is the mean of three specimens (standard deviations in Section 3). SEM–EDS observations (ASTM C1723) were made on fragments taken from the 56-day compressive specimens of A1 and A4. Hydration was stopped by oven-drying the fragments at 105 ± 5°C for 24 h and letting them cool to room temperature in the oven. The dried fragments were coated with gold and examined in a Hitachi S-3400N SEM (Hitachi High-Technologies, Japan) at an accelerating voltage of 15.0 kV. EDS point analyses (wt.%) were acquired with the attached energy-dispersive spectrometer. The XRD patterns of the raw materials (Figure 2) were recorded on a Bruker D8 diffractometer (Bruker AXS GmbH, Germany) with a position-sensitive detector, using Cu Kα radiation (λ = 1.5406 Å) at 40 kV and 40 mA, over 10°–80° 2θ with a step size of 0.05°. XRD of the hardened pastes was performed on mixtures A1, B1, C1 and D1 (s/b = 1.00) at an age of 56 days under the same conditions: after the drying procedure described above, the fine aggregate was removed and the paste was ground to pass a No. 200 (75 μm) sieve.

Figure 8

Simulated appearance of printed specimen.

2.3.3. Statistical analysis

Relationships between pairs of variables were evaluated by ordinary least-squares linear regression on the 16 mixture means, reporting the coefficient of determination (R 2), the p-value of the slope (two-sided t-test) and, where relevant, the 95% confidence interval (CI) of the slope. The main effects of the three independent design factors, which formed a full factorial with one mixture per cell, were tested by three-way analysis of variance (ANOVA) on the mixture means, with the interaction terms pooled into the error term (10 degrees of freedom); two-factor interactions were checked against the three-factor interaction (3 degrees of freedom), a test of limited power [51]. Partial eta-squared (η p 2) was used as the effect size and p < 0.05 as the significance level. Multiple linear regression with s/b, FM and CFA content as continuous predictors was used as a check.

3. Results and discussion

3.1. Printability

Printability was evaluated using flowability and mini-slump tests as practical proxies for the complex rheological properties required for additive manufacturing [52–54], with results summarized in Table 4. A two-stage methodology was employed. Stage I assessed the 16 mix designs at a fixed w/b of 0.55 against the printability criteria adopted here (mini-slump of 5.0–10.0 cm and fluidity >110 mm) [55]. In Stage II, the w/b (0.48–0.55) and superplasticizer (SP, 0.05%–0.10%) were adjusted so that every mixture fell within the same target mini-slump range of 5.0–10.0 cm, that the fresh state at printing was nominally common to all mixtures; because w/b and SP co-varied with s/b and FM (Table 4), the aggregate skeleton is regarded as the primary rather than the sole design variable. Flowability characterized workability, pumpability, and extrudability [56], exhibiting an inverse correlation with dynamic yield stress and plastic viscosity [55]. Conversely, the mini-slump test evaluated shape retention, indicating static yield stress and initial buildability [38].

Table 4

Printability of cementless mortar.

Mix no.s/bFMPrintability for stage IPrintability for stage II
w/bFlowability (mm)Mini slump (cm)w/bSP by binder (%)Flowability (mm)Mini slump (cm)Printed layers
A11.001.20.5515011.00.50—1507.511
A21.2515010.00.54—1508.511
A31.501506.50.55—1506.511
A41.751224.50.550.051506.715
B11.001.715012.20.48—1387.811
B21.2515010.80.53—1509.06
B31.501507.50.55—1507.511
B41.751305.50.550.051316.019
C11.001.215010.00.53—1509.06
C21.2515010.00.53—1507.210
C31.501326.00.53—1326.010
C41.751144.20.530.051507.012
D11.001.715012.20.49—1357.212
D21.2515010.00.52—1388.211
D31.501508.40.55—1508.415
D41.751295.00.550.101507.513

The s/b predominantly influenced fresh properties. Increasing the s/b from 1.00 to 1.75 decreased the mini-slump in every series and reduced flowability at s/b ≥1.50 due to a higher solid volume fraction and increased interparticle friction, which is known to raise yield stress and plastic viscosity [31,32]. However, this influence depended on a critical paste volume. In series A, flowability remained stable up to an s/b of 1.50 but collapsed abruptly at 1.75. Beyond this threshold, the paste volume was insufficient to lubricate the high specific surface area (SSA) of the fine aggregates, necessitating compensatory increases in w/b and SP to maintain workability and prevent extrusion blockage [31,32,39].

Aggregate fineness also affected printability. At equivalent s/b, mixtures with coarser sand (FM of 1.7) exhibited equal or higher flowability and mini-slump values than those with finer sand, an effect attributable to differences in SSA and particle packing [57]. Finer sand had a higher SSA, requiring more water to wet particle surfaces, thereby immobilizing free water and increasing effective yield stress and viscosity [30,31]. Consequently, coarser sand mixtures were more robust, permitting higher aggregate proportions while maintaining workability and reducing the required binder volume [58].

Regarding binder composition, all mixtures used a ternary blend containing 60% GGBS, with CFA acting as an internal activator and no external alkaline activator [16]. Replacing 5% of the spherical FA [59] with porous, irregular CFA [48] lowered the Stage I flowability at s/b ≥ 1.50, most clearly in the fine-sand series (C3: 132 mm against A3: 150 mm; C4: 114 mm against A4: 122 mm), whereas the differences at lower s/b were negligible. This is consistent with the higher water demand of irregular, porous CFA particles; viscosity was not measured, but the result indicates that FA and CFA should not be treated as interchangeable when printability is specified.

Actual buildability was assessed from the maximum number of printed layers (Table 4). Although all mixtures satisfied the target mini-slump range, stacking performance varied threefold, from 6 layers (Mixes B2 and C1) to 19 layers (Mix B4). The correlation between the mini-slump measured immediately after mixing and the number of stacked layers was weak (R 2 = 0.32, p = 0.021), and the residual scatter was large enough to be decisive in practice: B4 and C3 shared an identical mini-slump of 6.0 cm yet reached 19 and 10 layers, respectively, while B2 and C1 both lay at the upper bound of the window and failed after six layers. A single shape-retention measurement therefore did not describe stacking capacity. Mixtures at the highest s/b of 1.75 achieved the tallest builds in series A, B and C and the second tallest in series D (13 layers against 15 for D3), which is consistent with a denser granular skeleton contributing to green strength [32,39]; green strength and thixotropic recovery were, however, not measured directly. Whether that skeleton or the structuration kinetics of the binder was the operative variable is examined in Section 3.2.

3.2. Setting time

An assessment of the initial and final setting times for the 16 mixtures was conducted (Figure 9). All mixtures exhibited extended setting times, the fastest initial set occurring at 276 min (Mix C4) and 279 min (Mix A4) and the slowest at 409 min (Mix B2) and 407 min (Mix D2), consistent with the self-activated GGBS-CFA cementless binder system. Final setting followed the same ordering and ranged from 406 to 493 min.

Figure 9

Initial and final setting times of the mixtures.

The variations were associated mainly with aggregate fineness and s/b. Fine sand gave shorter setting times than coarse sand (mean initial set 318 against 369 min; ANOVA p = 0.004), and the highest s/b gave the shortest setting (304 min at s/b = 1.75 against 347 min at s/b = 1.00; p = 0.034 for s/b), consistent with the larger total specific surface area of finer and more abundant sand providing additional nucleation sites for hydration products [60,61] (e.g. Mix A1: 381 min versus Mix A4: 279 min; Mix C3: 289 min versus Mix D3: 393 min). Consequently, the fastest mixtures (A4, C4) combined fine sand with a high aggregate volume. Raising CFA from 30% to 35% shortened the setting time in the fine-sand series (Mix C1: 308 min versus Mix A1: 381 min), as expected from the greater supply of activating compounds [49,62,63], but averaged over all mixtures the reduction (351–336 min) was not significant (p = 0.31). A regression on s/b and FM described the setting behavior moderately well (R 2 = 0.52, p = 0.008), with FM the significant term (p = 0.007) and s/b marginal (p = 0.063).

Because these setting times were an order of magnitude longer than those of Portland-cement printing mortars, slow setting might be expected to limit stacking. Whereas mini-slump was a weak predictor of layer count (Figure 10a), initial setting time was unrelated to it (Figure 10b; R 2 = 0.04, p = 0.43), and the fastest-setting mixtures were not the tallest builds (C4: 276 min, 12 layers; B4: 312 min, 19 layers). Over the 276–409 min range, every mixture remained far from initial set during deposition, so the Vicat setting time did not discriminate between the mixtures. Stacking capacity instead increased with s/b (Figure 10c; R 2 = 0.36, p = 0.014; slope 6.6 layers per unit s/b, 95% CI 1.6–11.6), from a mean of 10.0 layers at s/b = 1.00 to 14.8 at 1.75. Adding FM raised the explained variance to 0.42, but the FM term was not significant (p = 0.27), and binder composition had no detectable effect. These observations are consistent with inter-particle contact in the fresh skeleton contributing to stacking capacity beyond what mini-slump or setting time captured, but they do not establish a mechanism: mini-slump and flow tests do not measure static yield stress, thixotropy or structural build-up [37,38], and more than half of the variance in layer count remained unexplained. Rheometric measurements would be needed to determine whether the skeleton acts through yield stress, build-up, or the frictional contact network.

Figure 10

Predictors of stacking capacity: (a) printed layers versus mini-slump; (b) printed layers versus initial setting time; (c) printed layers versus sand-to-binder ratio.

3.3. Compressive strength

The 56-day axial (X-direction) and lateral (Y-direction) compressive strengths, previously reported in [27], are reproduced in Table 5 to derive V p, AI, and k. All mixtures exceeded 20 MPa at 56 days, indicating effective self-activated hydration. CFA is expected to act as the principal internal activator [17]: its free lime hydrates to Ca(OH)2, raising the pH and dissolving the glassy GGBS [17,64], while dissolved anhydrite supplies sulfate for the precipitation of ettringite (AFt), a well-established route to early strength in sulfate-activated slag systems [17,64,65,66]. FA can then consume Ca(OH)2 in a pozzolanic reaction to form additional C–S–H [67], a plausible contributor to the strength gain observed between 28 and 56 days in some mixtures.

Table 5

Derived skeleton and performance parameters of the sixteen printed mixtures.

Mix no.s/bFMw/b V p f ax (MPa) f lat (MPa)AI f f (MPa) k
A11.001.20.500.68828.65 (0.47)17.74 (0.08)0.6193.53 (0.22)0.659
A21.251.20.540.64927.27 (0.65)13.91 (0.17)0.5104.33 (0.20)0.829
A31.501.20.550.60925.12 (0.55)14.61 (0.37)0.5824.70 (0.79)0.938
A41.751.20.550.57122.84 (0.87)14.75 (0.11)0.6464.73 (0.93)0.990
B11.001.70.480.68328.01 (0.94)16.44 (0.48)0.5874.89 (0.21)0.924
B21.251.70.530.64623.85 (0.90)18.43 (0.24)0.7734.05 (0.77)0.829
B31.501.70.550.60921.01 (0.81)17.09 (0.06)0.8135.21 (0.45)1.137
B41.751.70.550.57124.85 (0.53)15.64 (0.37)0.6296.09 (0.65)1.222
C11.001.20.530.69426.97 (0.97)19.46 (0.06)0.7224.13 (0.46)0.795
C21.251.20.530.64526.44 (0.51)17.71 (0.54)0.6704.76 (0.14)0.926
C31.501.20.530.60220.65 (0.31)13.29 (0.10)0.6443.49 (0.16)0.768
C41.751.20.530.56523.86 (0.06)15.48 (0.12)0.6493.95 (0.33)0.809
D11.001.70.490.68426.33 (0.39)20.10 (0.14)0.7635.99 (0.90)1.167
D21.251.70.520.64225.53 (0.19)14.70 (0.44)0.5764.77 (0.36)0.944
D31.501.70.550.60723.73 (0.12)16.10 (0.15)0.6786.05 (0.48)1.242
D41.751.70.550.57021.29 (0.25)16.07 (0.07)0.7555.67 (0.08)1.229
Mean———0.62724.7716.340.6634.770.963

Note: All values are at 56 days; strengths are means of three specimens, with standard deviations in parentheses.

Figure 11 shows strength development from 7 to 56 days. On average the mixtures reached 70% of their 56-day axial strength at 7 days (13.4–21.0 MPa) and 95% at 28 days (19.8–27.2 MPa), a rapid early gain for a binder without an external activator. Between 28 and 56 days, the axial strength increased significantly (t-test, p < 0.05, n = 3) in seven mixtures, by up to 27% (A3), and did not change significantly in the other nine; the nominal decrease of A4 (24.65–22.84 MPa, p = 0.086) lies within the specimen variability. The lateral strength developed in parallel (71% and 91% of its 56-day value at 7 and 28 days) and still increased between 28 and 56 days in twelve mixtures, so that the mean anisotropy index remained essentially constant (0.67, 0.64 and 0.66 at 7, 28 and 56 days; paired t-tests, p ≥ 0.11; Figure 11c). The effect of s/b on axial strength emerged with age: it was absent at 7 days (R 2 = 0.00, p = 0.84) but significant at 28 days (R 2 = 0.42, p = 0.007) and 56 days (R 2 = 0.55, p < 0.001), suggesting that early strength depends mainly on binder activation.

Figure 11

Development of the compressive strength of the printed specimens from 7 to 56 days: (a) axial (X-direction); (b) lateral (Y-direction); (c) anisotropy index (error bars: ± one standard deviation, n = 3).

An inverse correlation was identified between s/b and the 56-day axial compressive strength (R 2 = 0.55, p < 0.001), which was attributed to paste dilution [68]: a higher s/b reduces the volume of paste available to coat the aggregate particles and fill the inter-granular voids [69], producing a more porous matrix [70]. This effect could not be separated from the water demand imposed by the iso-workability constraint, because w/b was raised to preserve extrudability as the aggregate surface area and interparticle friction increased (Table 4) [57,71], generating a more interconnected capillary pore network [72]. The two variables were therefore combined into the paste volume fraction, V p = (V binder + V water)/(V binder + V water + V sand), which ranged from 0.565 to 0.694 (Table 5). V p gave the closest single-parameter description of axial strength (Figure 12; fax = 41.2V p − 1.0, R 2 = 0.57, p < 0.001; 95% CI of the slope 20.6–61.7 MPa), clearly better than w/b (R 2 = 0.38, p = 0.010) but only marginally better than s/b, with which it was almost collinear (R 2 = 0.99); V p is preferred because it also accounts for the w/b adjustment and has a direct physical meaning. The mould-cast reference cubes showed the same dilution effect at 56 days (versus s/b: R 2 = 0.35, p = 0.016; versus V p: R 2 = 0.34, p = 0.018), indicating that this is a property of the mortar rather than a printing artifact. Fitted by series (Figure 12), the relationship was strong for A (R 2 = 0.99, p = 0.006) and D (R 2 = 0.94, p = 0.030) but not significant for B (R 2 = 0.30) and C (R 2 = 0.49; n = 4 each). This was mainly because B3 and C3 (s/b = 1.50) lay about 3 MPa below the pooled line and B4 and C4 (s/b = 1.75) lay 1.6–2.4 MPa above it. As A and D differ in both sand and binder, as do B and C, this difference cannot be assigned to a single constituent; no s/b × FM or s/b × binder interaction was detected (p = 0.94 and 0.93; Section 3.6), and fits pooled by sand or by binder were all significant (R 2 = 0.53–0.65, p ≤ 0.042). The constant w/b of series C (0.53), in which V p varied only through sand dilution, may also contribute. Hence, V p is a proportioning guide within the investigated range rather than a predictive model.

Figure 12

Relationship between the 56-day axial compressive strength and the paste volume fraction, with pooled and series-specific linear fits (shaded band: 95% confidence interval of the pooled fit).

When comparing aggregate fineness at equivalent s/b, mixtures with fine sand (FM = 1.2, series A and C) gave a slightly higher mean 56-day compressive strength than those with coarser sand (FM = 1.7, series B and D), 25.22 against 24.32 MPa, but the difference was not significant (p = 0.28) and the ordering reversed for individual pairs such as C3 and D3. Finer sand may improve particle packing and reduce total porosity [73], thereby strengthening the ITZ [74,75] and partly offsetting its higher water demand [57].

Lateral compressive strength was lower than the axial value for every mixture because the printed interfaces acted as planes of weakness [40,41]. The mould-cast cubes provide a reference unaffected by printing (Figure 13a): at 56 days the printed axial strength did not differ from the cast strength (mean ratio 0.98, range 0.86–1.22; paired t-test, p = 0.32), whereas the lateral strength averaged 0.65 of it (0.52–0.82). At 28 days, the printed axial strength was slightly lower (ratio 0.95, p = 0.026), so the printed material had caught up by 56 days. Thus, strength loss in the printed elements was confined to loading across the interfaces, and the printed-to-cast ratios were not significantly affected by s/b or binder composition (p ≥ 0.27), with FM having a marginal effect (p = 0.059). Lateral strength varied over a narrower range than axial strength (13.29–20.10 MPa, SD 1.96 MPa, against 20.65–28.65 MPa, SD 2.48 MPa) and was only weakly related to it (Figure 13b; R 2 = 0.12, p = 0.18), but it decreased with s/b (R 2 = 0.33, p = 0.020; −3.9 MPa per unit s/b), an effect that was marginal in the factorial analysis (p = 0.079); FM and binder composition had no detectable effect. The anisotropy index, AI = f lat/f ax (Table 5), tended to decrease with increasing axial strength (Figure 13c; AI = −0.0160f ax + 1.06, R 2 = 0.23, p = 0.062), from 0.81 (B3) to 0.51 (A2), with a mean of about 0.66. Still, neither this trend nor the effects of s/b, FM, and binder composition (p ≥ 0.15) were significant. The higher mean AI of the coarser sand (0.70 vs. 0.63), contrary to the expectation of better bonding in finer, paste-rich mixtures [73,74], was also not significant. Because AI also did not change between 7 and 56 days (Figure 11c), the strength reduction across the interfaces was established early and persisted as both bulk and interfaces gained strength. These results are consistent with an interfacial capacity that depends more on the deposition conditions, which were common to all mixtures, than on the bulk strength. Interlayer bond strength was not measured directly, so this interpretation remains to be verified by direct bond tests; if confirmed, lateral performance would be improved more effectively through the deposition interval, surface moisture control, or interfacial treatment [43,44] than through the aggregate skeleton.

Figure 13

Directional strength of the printed mortar at 56 days: (a) axial and lateral strength of the printed specimens versus the strength of mould-cast cubes; (b) lateral versus axial compressive strength; (c) anisotropy index versus axial compressive strength.

3.4. Flexural strength

Figure 14 presents the 56-day flexural strengths. Flexural strength did not decline linearly with increasing s/b. In the coarse-sand series, D fell from 5.99 MPa at s/b = 1.00 to 4.77 MPa at 1.25 before recovering to 6.05 MPa at 1.50, and B reached its maximum of 6.09 MPa at s/b = 1.75 despite the highest w/b of that series. In the fine-sand series, A rose from 3.53 to 4.73 MPa, while C varied from 3.49 to 4.76 MPa with no clear trend. A higher w/b at increased s/b reduced paste quality, whereas a larger aggregate fraction can promote crack deflection and bridging [70], particularly with coarser particles; overall, however, the effect of s/b on flexural strength was not significant (p = 0.60; Section 3.6).

Figure 14

Flexural strength of the mixtures at 56 days (error bars: ± one standard deviation, n = 3).

The influence of aggregate fineness was pronounced and consistent. Mixtures prepared with the coarser sand reached a mean flexural strength of 5.34 MPa against 4.20 MPa for the finer sand (Figure 15(a)), a 27% increase; FM alone explained 48% of the variance in flexural strength (p = 0.003) and was the only significant factor in the factorial analysis (p = 0.008, η p 2 = 0.53), consistent with the literature linking higher FM to improved flexural performance [76]. A greater contribution of coarser particles to crack deflection and aggregate interlock is a plausible explanation, although fracture surfaces were not examined. In compression, by contrast, the finer sand was marginally superior, but not significantly (25.22 against 24.32 MPa). Binder composition had no significant effect on flexural strength (p = 0.65), with pairwise comparisons pointing in opposite directions (D1 exceeded B1 by 22.5%, whereas A3 exceeded C3 by 34.7%). Flexural and compressive strength were thus associated with different mixture features: FM with the former, and s/b, via V p, with the latter.

Figure 15

Flexural behaviour at 56 days: (a) effect of aggregate fineness modulus; (b) flexural strength versus the square root of the axial compressive strength, with the mean k for each sand grading and the code-based and geopolymer reference values.

The 56-day flexural-to-compressive strength ratios ranged from 12.3 to 26.6% with a mean of 19.5%, above the 10%–15% reported for comparable geopolymer systems [46]. Expressed through f f = k√f ax, k averaged 0.96 (95% CI 0.87–1.06) and ranged from 0.66 (A1) to 1.24 (D3) (Table 5 and Figure 15(b)). Because flexural strength depended on FM, k differed systematically between the sand gradings: 0.85 and 0.82 for series A and C and 1.03 and 1.15 for series B and D, i.e. 0.84 (95% CI 0.75–0.93) at FM 1.2 against 1.09 (95% CI 0.95–1.22) at FM 1.7 (p = 0.003). Series D thus exceeded the pooled mean, with three of its four mixtures above 1.16, and k is reported separately for each grading. Flexural strength was not correlated with compressive strength, either overall (R 2 = 0.02, p = 0.61) or within each grading (|r| = 0.08), so k is a descriptive ratio for this binder family rather than a transfer function. Figure 15(b) shows the values of 0.62 implied by ACI 318 [47] and 0.477 reported for geopolymer concrete [46] for reference only. The ACI relationship applies to the modulus of rupture of larger conventional beams in terms of cylinder strength. In contrast, the present values were obtained on 40 × 40 × 160 mm printed prisms in terms of 50 mm cube strength.

3.5. Microscopic analysis

Figure 16 and the corresponding EDS point analyses in Table 6 illustrate the microstructure of mixtures A1 and A4. These share the same binder (60% GGBS–30% CFA–10% FA) and sand (FM = 1.2) and differ only in s/b (1.00 and 1.75), thus bracketing the s/b range and spanning the largest strength difference within series A (28.65 and 22.84 MPa). These observations illustrate the effect of s/b within one series. The phase assignments below are tentative, as EDS has limited ability to resolve AFm, AFt, and C-A-S-H intermixed at the micrometer scale or to distinguish portlandite from Ca-rich amorphous or carbonated products.

Figure 16

SEM photos for A1 and A4 specimens (phase labels indicate tentative assignments based on morphology and EDS). (a) A1 specimen (×3,000), (b) A1 specimen (×5,000), (c) A4 specimen (×3,000), (d) A4 specimen (×10,000), (e) unreacted FA in A4 (×5,000).

Table 6

EDS results for A1 and A4 specimens (wt.%).

ElementContent (wt.%)
A1 from Figure 16a A1 from Figure 16b A4 from Figure 16c
Ca32.4521.8242.87
Si7.2410.304.75
Al3.064.66—
S1.433.45—
O55.8259.7752.38

At 3,000× (Figure 16a), the A1 fracture surface showed an irregular, blocky matrix with localized short needle-like crystals. EDS from these regions gave Ca (32.45%), Si (7.24%), Al (3.06%) and S (1.43%), a composition consistent with an intimate mixture of C-A-S-H gel and an AFm-type phase. At 5,000× (Figure 16b), abundant slender acicular crystals were observed; their higher S (3.45%) and Al (4.66%) contents and needle morphology are consistent with ettringite (AFt), which is expected in a sulfate-bearing CFA system [17,66]. Ettringite growth into capillary voids may have refined the pores.

Figures 16c and d show that A4 contained a block-like region with sharp boundaries and no evident needle- or gel-like products. EDS showed high Ca (42.87%) and low Si (4.75%), with Al and S below detection limits, giving a Ca/Si atomic ratio of about 6.3 (9.0 by mass), far above typical C-S-H values (about 1.75) [77]. Its Ca/O mass ratio (0.82) is close to calcite (0.83) and well below portlandite (1.25). Together with the abundance of calcite and scarcity of portlandite in the hardened pastes (Figure 17), this suggests calcite formed by carbonation during air curing or was inherited from the CFA, although this identification remains tentative because oxygen is only semi-quantitative in EDS and carbon was not analyzed. If poorly bonded to the matrix, such a coarse Ca-rich region could act as a weak inclusion; microcracks were observed adjacent to it (Figure 16d). Unreacted spherical FA particles also remained visible (Figure 16e), indicating incomplete pozzolanic reaction. These features may contribute to the lower strength of A4, although at the matrix scale the A1–A4 difference can be described by the lower V p of A4.

Figure 17

XRD patterns of the hardened paste fraction of mixtures A1, B1, C1 and D1, compared with the raw CFA.

XRD patterns of the paste fraction of the four mixtures with s/b = 1.00 (A1, B1, C1 and D1), covering both binders and both sand gradings, are shown in Figure 17. All four were dominated by quartz, probably from the FA and CFA (Figure 2) and from fine sand particles that passed the 75 μm sieve, which also account for the feldspar reflections at about 27.6°–28.1° 2θ (strongest in C1). Calcite, probably from the CFA and from carbonation during air curing, was the second main phase, and a broad hump at about 25°–35° 2θ was attributed to poorly crystalline C-(A)-S-H gel and residual slag glass. Weak portlandite reflections (about 18.1° and 34.2° 2θ) appeared in B1, C1 and D1 but not in A1. The anhydrite and lime reflections of the raw CFA (25.5° and 37.4° 2θ) were no longer detectable in any paste, indicating that the free lime and anhydrite had been largely consumed by the self-activation reactions, at least to below the XRD detection limit (Section 3.3). The four patterns were qualitatively similar, consistent with the absence of a significant binder effect on the mechanical properties (Section 3.6).

Ettringite and AFm reflections could not be distinguished from the background. This does not exclude their presence, because their strongest reflections lie below the 10° 2θ scan start, and oven-drying at 105 °C dehydrates these phases [78]; therefore, the XRD data neither confirm nor contradict the AFt and AFm assignments from SEM–EDS in A1, which remain tentative.

3.6. Statistical separation of design factors

Table 7 summarizes the factorial analysis. s/b was the only factor with a significant effect on f ax (p = 0.004, η p 2 = 0.72); its effects on layer count (p = 0.073) and f lat (p = 0.079) were marginal when s/b was treated as a four-level factor but significant as a linear trend (p = 0.014 and 0.020). FM was the only factor with a significant effect on f f (p = 0.008) and k (p = 0.003), and it also affected the initial setting time (p = 0.004; s/b p = 0.034). Binder composition had no significant effect on any response (p ≥ 0.30), and no factor affected AI (p ≥ 0.15). Except for FM × binder for initial setting time (p = 0.023), no two-factor interaction was significant. However, the low power of this test (three degrees of freedom) means that moderate interactions cannot be excluded. Multiple regression with continuous predictors gave the same pattern (fax: s/b p = 0.001; f f: FM p = 0.004; layer count: s/b p = 0.017).

Table 7

Three-way ANOVA (main effects) of the design factors on the measured and derived responses.

Responses/b: p (ηp 2)FM: p (η p 2)Binder: p (η p 2)Model R 2
Printed layers0.073 (0.49)0.287 (0.11)0.587 (0.03)0.52
Initial setting time 0.034 (0.56) 0.004 (0.59) 0.315 (0.10)0.74
f ax 0.004 (0.72) 0.276 (0.12)0.302 (0.11)0.74
f lat 0.079 (0.48)0.277 (0.12)0.532 (0.04)0.52
AI0.866 (0.07)0.155 (0.19)0.413 (0.07)0.28
f f 0.601 (0.16) 0.008 (0.53) 0.650 (0.02)0.57
k 0.150 (0.40) 0.003 (0.61) 0.495 (0.05)0.70

Note: Main-effects ANOVA on the 16 mixture means; η p 2, partial eta-squared; bold values, p < 0.05.

Two caveats apply to this analysis. First, w/b and SP were confounded with s/b and FM through the iso-workability adjustment, which is why V p was used as the descriptor in Section 3.3. Second, the analysis used mixture means, and the explained variances of 0.28–0.74 show that the three design factors capture only a fraction of the between-mixture variance. The analysis therefore identifies which property each design parameter mainly acts on rather than providing predictive models.

4. Conclusions

Based on the investigation of the 3D-printed self-activated cementless mortar, the following conclusions were drawn:

  1. A two-stage iso-workability procedure brought all 16 mixtures into one printing window (flow > 110 mm; mini-slump 5.0 to 10.0 cm), in which w/b and SP were adjusted as dependent variables. Stacking capacity nevertheless varied from 6 to 19 layers; mixtures with the same 6.0 cm mini-slump reached 10 and 19 layers, and mini-slump explained only 32% of the variance in layer count.

  2. Initial setting times ranged from 276 to 409 min and were shorter with finer sand (p = 0.004) and higher s/b (p = 0.034); binder composition had no significant effect. Setting time was not associated with stacking capacity (R 2 = 0.04, p = 0.43).

  3. Layer count increased with s/b (R 2 = 0.36, p = 0.014), whereas FM and binder composition had no significant effect. This is consistent with inter-particle contact in the fresh skeleton contributing to buildability. Still, because yield stress, thixotropy, and structural build-up were not measured, rheometry is needed to confirm the mechanism.

  4. V p gave the best single-parameter description of the 56-day axial compressive strength (f ax = 41.2 V p − 1.0; R 2 = 0.57, p < 0.001), marginally better than s/b (R 2 = 0.55) and clearly better than w/b (R 2 = 0.38). The fit was strong for series A and D (R 2 ≥ 0.94) and weak for series B and C. All mixtures exceeded 20 MPa at 56 days and reached, on average, 70% and 95% of this value at 7 and 28 days, respectively. V p is therefore a useful proportioning guide but not a predictive model.

  5. Printed specimens matched mould-cast cubes in axial strength (mean ratio 0.98, p = 0.32) but reached only 0.65 of their strength in the lateral direction, so the strength loss was confined to loading across the interfaces. Lateral strength was only weakly related to axial strength (R 2 = 0.12) and decreased moderately with s/b (p = 0.020). The anisotropy index ranged from 0.51 to 0.81 at 56 days, did not change significantly between 7 and 56 days, and was not significantly affected by s/b, FM or binder composition. These results suggest that interfacial capacity was set mainly by the common deposition conditions, which remains to be confirmed by direct interlayer bond tests.

  6. FM was the only design factor with a significant effect on flexural strength (5.34 against 4.20 MPa at FM 1.7 and 1.2; p = 0.008), and flexural strength was not correlated with compressive strength. The coefficient k in f f = k√f ax was 0.84 for FM 1.2 and 1.09 for FM 1.7.

  7. XRD of the paste fraction of A1, B1, C1 and D1 indicated that the anhydrite and free lime of the CFA had been consumed, leaving calcite, minor portlandite, and an amorphous gel hump; the four binders gave qualitatively similar patterns. SEM–EDS showed needle-like products consistent with ettringite and AFm/C-A-S-H in A1, and Ca-rich regions in A4 more consistent with calcite than with portlandite, along with unreacted fly ash.

The main limitations of the study are that the fresh state was characterized by mini-slump and flow tests rather than by rheometry, that interlayer bond strength was not measured directly, and that phase identification relied on SEM–EDS of two mixtures and on XRD of oven-dried pastes scanned from 10° 2θ, which could not resolve ettringite or AFm phases. Rheometric measurement of the static yield stress and structural build-up, direct interlayer bond tests, and low-angle XRD after solvent exchange combined with thermogravimetric analysis are recommended to test the interpretations proposed here.

Nomenclature

Abbreviations

3DCP, 3D

concrete printing

AAM

alkali-activated material

AFm

monosulfate-type calcium aluminate hydrate

Aft

ettringite

AI

anisotropy index

ANOVA

analysis of variance

C-A-S-H

calcium aluminosilicate hydrate

C-S-H

calcium silicate hydrate

CFA

co-fired fly ash

CFB

circulating fluidized bed

CI

confidence interval

CM

cementless mortar

COV

coefficient of variation

EDS

energy-dispersive X-ray spectroscopy

FA

fly ash

FM

fineness modulus

GGBS

ground granulated blast-furnace slag

ITZ

interfacial transition zone

OPC

ordinary Portland cement

SD

standard deviation

SEM

scanning electron microscopy

SP

superplasticizer

SSA

specific surface area

SSD

saturated-surface-dry

XRD

X-ray diffraction.

Symbols

f ax

56-day compressive strength in the axial (X) direction (MPa)

f lat

56-day compressive strength in the lateral (Y) direction (MPa)

f f

56-day flexural strength (MPa)

AI = f lat/f ax; k

flexural–compressive coefficient, k = f f/√f ax (MPa0.5)

s/b

sand-to-binder mass ratio

w/b

water-to-binder mass ratio

V p

paste volume fraction

V binder, V water, V sand

absolute volumes of binder, water and sand

R 2

coefficient of determination

p

probability value

η p 2

partial eta-squared

n

number of mixtures.

Acknowledgement

The authors want to acknowledge the National Science and Technology Council in Taiwan under Grant NSTC-114-2221-E-197-001-MY2.

Author contributions

Jie Chen: conceptualization, writing-original draft preparation, writing-review and editing. Kinga Korniejenko: validation, writing-review and editing. Chia-Ying Ho: data curation, investigation, writing-original draft preparation. Wei-Ting Lin: methodology, resources, writing-original draft preparation, writing-review and editing, project administration.

Conflict of interest statement

Authors state no conflict of interest.

DOI: https://doi.org/10.2478/msp-2026-0022 | Journal eISSN: 2083-134X (formerly 2083-124X) | Journal ISSN: 2083-1331
Language: English
Page range: 126 - 148
Submitted on: Aug 17, 2026
Accepted on: Oct 24, 2026
Published on: Nov 16, 2026
Published by: Wroclaw University of Science and Technology
In partnership with: Paradigm Publishing Services

© 2026 Jie Chen, Kinga Korniejenko, Chia-Ying Ho, Wei-Ting Lin, published by Wroclaw University of Science and Technology
This work is licensed under the Creative Commons Attribution-NonCommercial-NoDerivatives 4.0 License.