Skip to main content
Have a personal or library account? Click to login
Investigation and optimization process of powder-suspended electro-discharge machining for machining attributes of SKD11 steel Cover

Investigation and optimization process of powder-suspended electro-discharge machining for machining attributes of SKD11 steel

Open Access
|Oct 2026
Read online

Full article

1. Introduction

SKD11 steel is a high-alloy tool steel with a high carbon and chromium content, notable for its high hardness, superior wear resistance, good dimensional stability after heat treatment, and efficient performance under high load and friction conditions [1]. Owing to these properties, SKD11 is widely used in cold stamping dies, cutting dies, bending dies, metal cutting tools, and machine parts requiring a long service life and strict geometric accuracy. However, SKD11’s high hardness and strength also make it difficult to machine using traditional cutting methods; thus, electrical discharge machining (EDM) is a suitable technological solution. Despite this, machining efficiency is low, and surface quality is poor due to the thermal effects of the process. Recently, the incorporation of conductive powder into the solvent during the EDM process has shown great potential for improving machining efficiency and surface quality. This solution is called powder-mixed electrical discharge machining (PMEDM).

PMEDM has been studied for approximately four decades. For example, Erden et al. first reported on the effects of powders, including Fe, C, Al, and Cu, on machining performance, surface finish, and discharge characteristics in 1981 [2]. Subsequent research has investigated the impact of several powders on machining properties and surface quality, comprising Si, SiC, Gr, Ti, Mo, Cr, Al, TiC, Ni, C, and W [3]. Numerous workpiece materials that are often used in industries have been studied, including SS304, SKD11 steel, SKD61 steel, titanium alloy, AISI P20 steel, and others [4,5].

PMEDM is a sophisticated advancement of conventional EDM that significantly enhances machining efficiency and surface integrity of hard-to-cut materials such as SKD11 die steel. This process involves mixing fine powders, such as aluminum, silicon carbide, or graphite, into the dielectric fluid, which reduces its insulating strength and expands the interelectrode gap [6]. In the context of machining SKD11, the research by Yan and Chen has demonstrated that the addition of aluminum and silicon carbide powders leads to a considerable improvement in the material removal rate (MRR) [7]. The underlying mechanism is often described as a “bridging effect,” where powder particles get energized and form chains under the sparking area, facilitating a more stable “series discharge.” This dispersion of energy prevents the spark from striking the workpiece directly, leading to the formation of shallower and more uniform craters compared with those produced by standard EDM [8]. Surface quality is a critical factor for SKD11 components, and PMEDM has shown remarkable results in refining surface roughness (SR). For instance, utilizing aluminum powder combined with a surfactant in the dielectric has been reported to improve the surface finish of SKD11 steel by as much as 60%, reducing R a values from 0.434 to 0.172 μm [1]. Surfactants (such as Span-20) play a vital role in ensuring a homogeneous suspension of the powder, which prevents particles from agglomerating or settling at the bottom of the tank [9]. This uniform distribution minimizes the “bridge effect” caused by overconcentration in one area, thereby enhancing the distribution of discharge energy and further improving MRR and tool wear rate (TWR) [10].

Despite the extensive research on PMEDM using different conductive powders and workpiece materials, several aspects remain insufficiently clarified. Previous investigations have primarily focused on evaluating the effects of powder addition and electrical parameters on individual machining responses, whereas a systematic integration of machining productivity, tool wear, and SR with multi-response optimization remains relatively limited for tungsten-powder-assisted PMEDM of SKD11 steel. In particular, the influence of the optimization framework itself on the resulting machining trade-offs has not been sufficiently discussed. This issue is important because different multi-objective optimization strategies may lead to different optimal parameter combinations even when the same experimental data and machining objectives are considered.

Consequently, it is important for both production and research to examine the machinability of SKD11 steel using EDM machining with tungsten powder alloy. Based on this, the impacts of machining parameters on machining attributes, comprising TWR, MRR, and SR-R a, are investigated in this study. Subsequently, the relationship between the various machining parameters (such as powder amount [A p], pulse-on time [T on], and peak current [I p]) and the machining characteristics (such as TWR, MRR, and R a) is established using mathematical models. Finally, the multi-objective optimization on the basis of ratio analysis (MOORA) and desirability approach (DA) are implemented the optimum problem concurrently for determining the minimal TWR and R a, and the maximal MRR to choose a reasonable solution for each machining attribute to ameliorate the machining features. Furthermore, the surface characteristics (defects and thickness of the recast layer) at the optimal settings of the two techniques are also taken into account. These help to increase understanding and knowledge of the EDM method, which processes SKD11 steel using tungsten powder alloy.

2. Empirical procedure and method

2.1. Materials

Due to its wide range of industrial applications and favorable machinability characteristics, SKD11 tool steel was selected as the workpiece material in this study. The material’s chemical makeup (weight percent) was 1.5% C, 0.5% Mn, 0.3% Si, 12% Cr, 0.35% V, and 1% Mo, with Fe making up the remaining percentage. Before conducting the experiments, the specimens were prepared by external turning and face grinding operations to ensure high geometric precision and dimensional accuracy. Cylindrical samples with dimensions of 50 mm in length and 20 mm in diameter were fabricated, with dimensional deviations among specimens controlled within 0.01 mm. The prepared samples are illustrated in Figure 1b.

Figure 1

Experimental diagram of the study.

A cylindrical copper electrode with 99% purity, a diameter of 25 mm, and a length of 50 mm (Figure 1c) was connected to the cathode of the CNC-460 EDM machine (Aristech) to conduct the machining experiments (Figure 1a). The dielectric medium was stored in a steel tank with an approximate volume of 0.05 m3 (415 mm × 330 mm × 350 mm). EDM Fluid 2, supplied by Shell, was used as the dielectric medium (Figure 1d). Tungsten powder alloy was added to the dielectric, with a compositional chemistry (wt.%) of 82.5% W, 5.56% C, 11.9% Co, 0.02% Fe, and 0.02% others (Figure 1e); its physical properties are indicated in Table 1, and the scanning electron microscopy (SEM) image is depicted in Figure 2.

Table 1

The physical properties of tungsten powder alloy.

Particle size distributionUpto 5.5 µmUp to 11 µmUp to 16 µmUp to 22 µmUp to 31 µm
5.23%25.98%59.74%89.35%98.93%
DensityApparent density: >6.8 g/cm3 Vibrating density: >8.2 g/cm3
Electrical conductivity132–522 (×104・Ω−1・m−1)
Figure 2

SEM of tungsten powder alloy.

A mechanical stirring system consisting of an electric motor, a stirring shaft, and impeller blades was installed inside the machining tank to ensure continuous agitation and maintain a homogeneous powder concentration throughout the entire machining process. This configuration prevents particle sedimentation and helps achieve stable machining conditions. After each experiment, the tungsten powder alloy is carefully filtered from the dielectric solution to avoid material loss and waste and to allow for reuse in subsequent experiments. The complete experimental setup and measurements are shown in Figure 1.

2.2. Basis for empirical selection and design

Among the electrical machining parameters, the discharge current (I p) and pulse-on time (T on) are widely recognized as having a significant influence on the machining performance characteristics of EDM processes. Therefore, these two parameters were selected as the primary electrical factors investigated in this study [11]. Meanwhile, the pulse-off time (T off) was fixed at 50 µs, the inter-electrode working gap was maintained at 210 µm, and the discharge voltage was maintained at 120 V, in accordance with the technical specifications recommended for the CNC-460 EDM machine. These parameters were kept constant throughout all experimental runs. In addition, the concentration of powder (A p) mixed into the dielectric fluid was carefully determined to ensure compatibility with the electrical and thermal conductivity characteristics of the powder, as well as its effective interaction with the selected voltage level. Consequently, the input parameters considered in this research include discharge current (I p), pulse-on time (T on), and powder concentration (A p), while the output responses are MRR, TWR, and SR (R a). To minimize the number of experimental trials while maintaining sufficient accuracy and reducing both experimental time and cost, an appropriate experimental design methodology was required. The experimental matrix was, therefore, developed based on the Box–Behnken design, which satisfies these requirements and is suitable for modeling nonlinear relationships among process variables. Accordingly, the Box–Behnken design was adopted in this study. The selected levels of the input parameters are presented in Table 2.

Table 2

Process parameter levels.

Process parametersLevel
I p (A)468
T on (µs)50100150
A p (g/L)0510

2.3. The process for identifying output responses

2.3.1. Surface roughness

The SR of the machined specimens (R a) was measured using a contact-type profilometer (SJ-201, Mitutoyo, Japan), as shown in Figure 1f, in accordance with the ISO 4287 standard. For each measurement, an evaluation length of 4 mm was used, consisting of five sampling lengths of 0.8 mm each. SR measurements were conducted at three equally spaced locations on the machined surface of each specimen. At every location, three repeated measurements were performed to ensure reliability. The final SR value was determined by averaging the repeated measurements at each location, followed by calculating the overall mean value of the three measured positions.

2.3.2. TWR and MRR

To evaluate MRR and TWR, the masses of both the workpiece and the electrode were measured before and after machining using a precision electronic balance (Sartorius TE214S, resolution of 0.0001 g) with three repetitions, as shown in Figure 1g. The MRR and TWR values were then calculated based on the mass difference according to equations (1) and (2), respectively. The final MRR and TWR values are determined by averaging the repeated measurements at each measurement.

The machining time was determined as the time required to machine the workpiece until its length was reduced by 0.5 mm (from 50 mm to 49.5 mm) during the PMEDM operation.

MRR is calculated using equation (1):

(1)
MRRmgmin=M1 − M2t,
where M 1 and M 2 represent the mass of the workpiece before and after machining, respectively, and t denotes the machining time.

Similarly, TWR is determined using equation (2):

(2)
TWRmgmin=m1 − m2t,
where m 1 and m 2 are the masses of the tool electrode before and after machining, respectively.

2.3.3. The recast layer

After machining, the specimens were sectioned perpendicular to the machined surface to obtain cross-sectional samples for metallographic observation. The samples were then prepared using standard metallographic procedures, including grinding with fine abrasive paper (grit size 2000), followed by polishing using a felt polishing wheel to obtain a smooth surface. The thickness of the recast layer on the machined surface was then observed and evaluated using an optical microscope (AXIO-A2M) (Figure 1i).

2.3.4. The defects of machined surfaces

Surface morphology and defects formed after machining processes were examined using SEM on the HITACHI SU3800 system (Figure 1i). These observations were used to evaluate the influence of machining conditions on surface integrity. In addition, a HITACHI SU3800 machine was used to determine the content, distribution, and elemental composition on surfaces by energy-dispersive X-ray spectroscopy (EDS).

2.4. Establishment of predictive models

A second-order (quadratic) regression model, as expressed in equation (3), was proposed to establish the relationship between the input parameters and the output responses (MRR, TWR, and R a):

(3)
y=β0+∑i=1nβixi+∑i=1nβiixi2+∑i<j∑j=2nβijxixj+δ,
where β 0 is the intercept term, β i , β ij , and β ij are the regression coefficients of the model, x i and x j represent the input (control) variables, n is the number of input variables (n = 3), δ denotes the residual error, and y represents the output response.

The experimental and measurement results obtained from the designed experiments are summarized in Table 3.

Table 3

The empirical matrix and the responses with standard deviation.

No.Processing parametersAttained responses
T on (µs) I p (A) A p (g/L)MRR (mg/min)TWR (mg/min) R a (µm)
11008104.3053 ± 0.06460.8248 ± 0.01072.34 ± 0.0257
2506103.5154 ± 0.04920.4642 ± 0.00511.82 ± 0.0146
350853.8630 ± 0.06570.8038 ± 0.00801.98 ± 0.0238
4150603.1463 ± 0.03460.7034 ± 0.01133.42 ± 0.0308
5100402.7448 ± 0.03290.4503 ± 0.00771.96 ± 0.0216
6100803.8545 ± 0.05400.9455 ± 0.01132.77 ± 0.0360
750602.8924 ± 0.02890.6331 ± 0.01012.36 ± 0.0260
81506103.6371 ± 0.06180.5633 ± 0.00733.45 ± 0.0311
9150854.0720 ± 0.05290.8297 ± 0.01003.28 ± 0.0394
1050452.7259 ± 0.03270.3119 ± 0.00471.32 ± 0.0172
11100653.1913 ± 0.04150.5759 ± 0.00752.18 ± 0.0218
12100653.1590 ± 0.03470.5719 ± 0.00802.19 ± 0.0197
131004103.4707 ± 0.03820.3451 ± 0.00452.02 ± 0.0182
14150453.2955 ± 0.04610.4345 ± 0.00702.64 ± 0.0264
15100653.1676 ± 0.04750.5791 ± 0.00752.17 ± 0.0239

2.5. Optimization with multiple objectives

Optimization plays an important role in improving both technical performance and economic efficiency in manufacturing processes. In the PMEDM process, machining productivity and surface quality must be simultaneously considered. In this study, the desired machining performance is defined as maximizing MRR while minimizing TWR and SR (R a). Achieving these objectives contributes to reducing machining time and improving dimensional accuracy and surface integrity of the machined components.

Accordingly, the multi-objective optimization problem in the PMEDM process can be formulated as follows:

Find x = [I p, T on, A p] for maximizing MRR and minimizing TWR and R a.

Subject to the following constraints: 4 ≤ I p ≤ 8 (A), 50 ≤ T on ≤ 150 (µs), and 0 ≤ A p ≤ 10 (g/L)

In this research, two multi-objective optimization methods, namely DA and MOORA, were employed to determine the optimal machining parameters. The obtained optimization results are then compared and evaluated.

2.5.1. Desirability approach

The DA is recognized as one of the most practical and efficient techniques for multi-response optimization. This method, introduced by Derringer and Suich (1980) [12,13], transforms each response value y i into a dimensionless desirability function d i , where the desirability scale ranges from 0 to 1. A value of d i = 0 represents a completely unacceptable outcome, while d i = 1 corresponds to the most desirable result.

For responses that must be minimized, the individual desirability is formulated according to equation (4), whereas for responses that are required to be maximized, the desirability is computed using equation (5). In both cases, the lower and upper bounds of the response variable are denoted by L and H, respectively. A positive parameter r (with r > 0) is introduced to adjust the shape of the desirability function, thereby controlling the emphasis placed on values closer to the target region.

(4)
di(yi)=0, yi<LH−yiH−Lr, L≤1, yi>Hyi≤H.
(5)
di(yi)=0, yi<Lyi−LH−Lr, L≤1, yi>Hyi≤H.

After calculating the individual desirability values for all responses, the overall desirability index D is obtained using equation (6). This index is determined as the weighted geometric mean of the individual desirabilities:

(6)
D=∏i=1nDiwi1∑wi,
where w i denotes the weight assigned to the i-th response (with w i > 0), and n represents the total number of response variables considered. The optimal solution is identified as the parameter combination that yields the maximum overall desirability value.

2.5.2. Multi-objective optimization on the basis of ratio analysis

The MOORA method is a multi-criteria decision-making approach used to rank alternatives according to multiple performance attributes [14]. The method evaluates beneficial and non-beneficial criteria simultaneously and provides a simple computational procedure for determining the optimal alternative.

The procedure of the MOORA method is described as follows:

First, the decision matrix is constructed:

(7)
X=[rij]m×n,
where r ij represents the performance value of the i-th alternative with respect to the j-th attribute, mmm is the number of alternatives, and nnn is the number of attributes.

Next, the decision matrix is normalized using vector normalization:

(8)
rij⁎=rij∑i=1mrij2,
where rij⁎ denotes the normalized value of the i-th alternative for the j-th attribute.

After normalization, the assessment value of each alternative is calculated using the attribute weights:

(9)
yi=∑j=1gwjrij⁎−∑j=g+1nwjrij⁎,
where g is the number of beneficial attributes, n − g is the number of non-beneficial attributes, and w j is the weight of the j-th attribute.

Finally, the alternatives are ranked in descending order according to y i . The alternative with the highest assessment value is considered the optimal solution.

2.5.3. Weight determination using the criteria importance through intercriteria correlation method

The weights of the output responses are determined using the criteria importance through intercriteria correlation (CRITIC) [15] method. Let the decision matrix be expressed as follows:

(10)
X = [xij], i =1,…, m; j = 1,…, n,
where m is the number of alternatives and n is the number of response attributes.

Normalization of the decision matrix: To eliminate dimensional differences among attributes, the decision matrix is normalized.

For a beneficial attribute:

(11)
xij=rij−min(rj)max(rj)−min(rj); i=1,..., m, j=1,..., n.
For a non-beneficial attribute:
(12)
xij=max(rj)−rijmax(rj)−min(rj); i=1,..., m, j=1,..., n,
where x ij is the normalized value.

Standard deviation of attributes: The contrast intensity of each attribute is measured by the standard deviation as follows:

(13)
σij=1n−1∑j=1n(xij−x¯j)2; i=1,..., m,
where x¯j is the mean value of the j-th attribute.

Correlation coefficient: The correlation coefficient between attributes j and k is calculated as follows:

(14)
ρjk=∑i=1m(xij−x¯j)(xik−x¯k)∑i=1m(xij−x¯j)2∑i=1m(xik−x¯)k2.
Information index: The amount of information contained in each attribute is defined as follows:
(15)
Cj=σj∑k=1n(1−ρjk); j=1,..., n
Weight calculation: Finally, the weight of each attribute is determined by:
(16)
wj=Cj∑j=1nCj;j=1,..., n.
These weights are then used in the subsequent MOORA and DA analyses.

3. Results and discussion

3.1. Impacts of the process variables on MRR

Based on the main effects plot for MRR as indicated in Figure 3a, the influence of each factor (I p, T on, and A p) on the MRR is observed as follows: I p shows the strongest effect on MRR among the three factors. As I p increases from 4 to 8 A, the mean MRR rises sharply (from about 3.05 to above 4.0 mg/min). The steep slope of the line indicates a high sensitivity of MRR to I p. This trend is physically reasonable in EDM/PMEDM processes, since higher peak current increases discharge energy [16], leading to more intense melting and vaporization of material, thereby significantly enhancing the MRR. Meanwhile, T on has a moderate and positive influence on MRR. An increase in T on from 50 to 150 µs results in a gradual increase in mean MRR (approximately from 3.25 to 3.55 mg/min). The slope is gentler than that of I p, which suggests that while longer pulse-on time allows more energy per discharge and promotes material erosion, its effect is less dominant than peak current. Excessively long T on may also approach a saturation region where further gains in MRR are limited. Finally, A p also exhibits a noticeable positive effect on MRR. As A p increases from 0 to 10 g/L, the mean MRR increases from roughly 3.15 to 3.7 mg/min. The slope is steeper than that of T on but still lower than I p, indicating that A p is the second most influential factor in this study. The improvement in MRR can be attributed to the presence of conductive powder particles, which enhance spark dispersion, enlarge the discharge gap, and facilitate more efficient material removal.

Figure 3

The main and interactive influence of process variables on MRR.

Figure 3b–d shows the integrated impacts of the process variables on MRR. According to Table 4, I p has the greatest impact on MRR with a contribution of 59.48%, followed by A p (20.96%) and T on (5.32%). When T on and I p are simultaneously increased throughout the whole A p study space, MRR increases, as shown in Figure 3b. As shown in Figure 3c and d, MRR increases when I p or T on are increased throughout the whole A p research space. According to the previously described analysis, an increase in T on and/or I p causes increased discharge energy, which raises MRR [17]. In addition, adding powder to the insulating solvent encourages stratified discharge, which raises MRR. The MRR findings from this investigation are consistent with those from earlier research [18].

3.2. Impacts of the process variables on TWR

The main effects of each process parameter on TWR are shown in Figure 4a. In there, I p has the most significant effect on TWR. As I p increases from 4 to 8 A, the mean TWR rises sharply from approximately 0.39 to 0.85 mg/min. The steep slope indicates that tool wear is highly sensitive to peak current. This behavior is expected, as higher I p increases discharge energy and plasma temperature, intensifying thermal loading on the tool electrode and accelerating its erosion. T on shows a moderate influence on TWR. Increasing T on from 50 to 150 µs leads to a gradual increase in TWR (from about 0.55 to 0.63 mg/min). The relatively gentle slope compared to I p suggests that longer discharge duration increases heat transfer to the tool, but its impact on tool wear is less dominant than peak current. A p exhibits a positive effect on the improvement of TWR. As A p increases from 0 to 10 g/L, the mean TWR decreases from around 0.68 to 0.55 mg/min. This downward trend indicates that higher powder concentration helps reduce tool wear. The presence of powder particles promotes uniform spark distribution, stabilizes discharges, and reduces localized overheating of the tool, thereby mitigating electrode erosion [18].

Figure 4

The main and interactive influence of process variables on TWR.

Figure 4b–d shows the interactive impacts of the process variables on TWR. According to Table 4, I p has the greatest impact on TWR with a contribution of 87.48%, followed by A p (7.22%) and T on (2.55%). The I p–T on surface clearly indicates a strong synergistic interaction, as shown in Figure 4b. TWR increases markedly when both I p and T on increase simultaneously. At low I p (4 A), increasing T on causes only a moderate rise in TWR. However, at higher I p levels (8 A), the same increase in T on leads to a much steeper increase in TWR. The curved surface and non-parallel contour lines confirm that the effect of T on on tool wear strongly depends on the level of I p. Physically, higher I p raises discharge energy density, and longer T on prolongs heat exposure, together intensifying thermal erosion of the tool electrode [19]. Meanwhile, the I p–A p interaction shows a significant but moderating effect of A p on tool wear, as indicated in Figure 4c. TWR increases sharply with increasing I p, regardless of A p level, confirming I p as the dominant factor. However, at higher A p values, the rate of increase in TWR with I p becomes slightly less steep. This indicates that powder concentration mitigates tool wear, even under high current conditions. The conductive powder particles help distribute discharges more uniformly and reduce localized overheating on the tool surface, thereby partially offsetting the wear caused by high I p [20]. Finally, the interaction of T on–A p exhibits a relatively weak. TWR increases gradually with T on, while increasing A p leads to a noticeable reduction in TWR. The surface is comparatively flatter, and the contour lines are more parallel, indicating that the influence of T on on TWR is largely independent of A p, and vice versa. This suggests a more additive rather than synergistic interaction between these two parameters.

3.3. Impacts of the process variables on R a

Based on the main effects plot for R a as depicted in Figure5a. In there, R a increases with increasing I p, rising from about 2.0 µm at 4 A to nearly 2.6 µm at 8 A. The upward trend indicates that higher peak current leads to rougher surfaces. This is due to the higher discharge energy at elevated I p, which forms larger and deeper craters on the machined surface. Although the increase from 6 A to 8 A is relatively mild compared with the jump from 4 to 6 A, I p still shows a clear positive influence on SR. Meanwhile, T on exhibits the strongest effect on R a among the three parameters. Increasing T on from 50 to 150 µs causes R a to increase sharply from approximately 1.9 to over 3.2 µm. The steep slope reflects the high sensitivity of SR to pulse duration. Longer T on allows each discharge to act for a longer time, which increases molten pool size and promotes the formation of coarser surface features and resolidified debris; the result is a significant degradation of surface finish [8]. Finally, A p shows a nonlinear influence on R a. Increasing A p from 0 to 5 g/L reduces R a from about 2.6 µm to 2.25 µm, indicating an improvement in surface finish. This can be attributed to improved spark dispersion and reduced discharge intensity due to the presence of powder particles [21]. However, further increasing A p to 10 g/L causes R a to increase slightly again, suggesting that excessive powder concentration may lead to unstable discharges or particle agglomeration, which deteriorates surface quality.

Figure 5

The main and interactive influence of process variables on R a.

Figure 5b–d shows the interactive impacts of the process variables on R a. According to Table 4, T on has the greatest impact on R a, with a contribution of 66.82%, followed by I p (13.99%) and A p (1.84%). The I p–T on surface (Figure 5b) shows a strong interaction effect on R a. R a increases significantly when both I p and T on increase simultaneously. At low I p (4 A), increasing T on causes only a moderate rise in R a. However, at higher I p (8 A), the same increase in T on leads to a much steeper increase in R a. The pronounced curvature and non-parallel contour lines indicate a synergistic interaction, where the influence of T on on R a is amplified by higher I p. Physically, high discharge energy (high I p) combined with long pulse duration (high T on) produces larger molten pools and deeper craters, resulting in a much rougher surface [21]. For the interactive influence of I p–A p, this relationship exhibits a moderate but noticeable effect. R a generally increases with increasing I p, confirming that peak current strongly governs crater size [22]. However, A p modifies this effect: at moderate A p levels, R a is reduced compared with A p = 0, particularly at lower I p. This suggests that powder particles help disperse the discharge energy and smooth the surface. At higher I p, the benefit of A p becomes less pronounced, indicating that excessive discharge energy dominates surface formation. The curved contours confirm that A p partially counteracts the roughening effect of I p but does not eliminate it. Finally, the T on–A p surface reveals a nonlinear interaction. R a increases strongly with T on, while A p exhibits an optimal region. At low to moderate A p, R a decreases, especially at shorter T on, leading to improved surface finish. However, at higher T on, R a increases even with increasing A p, indicating that long pulse duration overwhelms the beneficial effect of powder concentration. The bowl-shaped surface and curved contour lines indicate that A p can reduce R a only within a limited T on range.

Table 4

ANOVA for all the output results.

ResponsesMRRTWR R a
p-Value I p <0.0001<0.0001<0.0001
T on 0.00160.0022<0.0001
A p <0.00010.00020.0004
I p × T on 0.04030.05620.7982
I p × A p 0.08980.70790.0012
T on × A p 0.35960.49410.0006
I p 2 0.00030.01860.0002
T on 2 0.77660.1868<0.0001
A p 2 0.01990.0287<0.0001
Contribution I p 59.48%87.48%13.99%
T on 5.32%2.55%66.82%
A p 20.96%7.22%1.84%
I p × T on 1.039%0.47%0.002%
I p × A p 0.605%0.01%1.138%
T on × A p 0.14%0.04%1.54%
I p 2 10.31%0.88%3.6%
T on 2 0.0006%0.23%5.712%
A p 2 1.45%0.74%5.23%

Accuracy of the models: MRR: R 2 = 0.9932, adjusted R 2 = 0.9808, and predicted R 2 = 0.893; TWR: R 2 = 0.9961, adjusted R 2 = 0.9892, and predicted R 2 = 0.9391; R a: R 2 = 0.9987, adjusted R 2 = 0.9964, and predicted R 2 = 0.9797.

3.4. Develop predictive models and evaluate model adequacy

Regression modeling was performed in Minitab (version 22) to obtain the coefficients of the predictive equations for the response variables. The resulting models describing TWR, MRR, and R a are given in equations (17)–(19), respectively, as follows:

(17)
MRR (mg/min)=3.202−0.541Ip+0.00845Ton+0.0673Ap+0.07557Ip2+0.000003Ton2+0.00444Ap2−0.000901IpTon−0.00688IpAp−0.000132TonAp,
(18)
TWR (mg/min)=0.012+0,0362Ip+0.0033Ton−0.0265Ap+0.00885Ip2−0.000006Ton2+0.001258Ap2−0.000242IpTon−0.000387IpAp+0.000029TonAp,
(19)
Ra (μm)=−0.219+0.7706Ip−0.01374Ton−0.1148Ap−0.04604Ip2+0.000122Ton2+0.010933Ap2−0.00005IpTon−0.01225IpAp+0.000570TonAp.
The adequacy and significance of the developed models were evaluated using analysis of variance (ANOVA) at a 95% confidence level (significance level of 0.05). The ANOVA results are summarized in Table 4. Furthermore, the normal probability plots of residuals for MRR, TWR, and R a (Figure 6a–c) indicate that the standardized residuals are approximately aligned along a straight line, confirming that the residuals follow a normal distribution. This observation demonstrates the statistical adequacy and reliability of the developed regression models. Based on these statistical validation results, the predictive models for TWR, MRR, and R a are considered sufficiently accurate within the experimental design space and can be used for optimization and response prediction.

Figure 6

The normal probability plot.

3.5. The optimum findings

As described previously, this study employs two multi-objective optimization methods, namely DA and MOORA, to solve the optimization problem. The weights of the three response characteristics were determined using the CRITIC method based on the normalized decision matrix and intercriteria correlation. The obtained weights are w 1 = 0.43693 for MRR, w 2 = 0.30625 for TWR, and w 3 = 0.25682 for R a. These weights were subsequently incorporated into both the DA and MOORA procedures to evaluate the overall performance of the experimental runs.

3.5.1. Optimization findings of DA

In DA, the relative importance of the responses MRR, TWR, and R a is represented by the weighting factors w 1, w 2, and w 3, respectively. Based on this weighted multi-response optimization, the DA method identified the optimal machining parameters as I p = 8 A, T on = 50 µs, and A p = 10 g/L, yielding an overall desirability value of D = 0.864.

Under these optimal conditions, the predicted performance characteristics were MRR = 4.117 mg/min, TWR = 0.7159 mg/min, and R a = 1.87 µm. These values represent the best compromise solution obtained from the simultaneous consideration of maximizing MRR while minimizing TWR and SR.

3.5.2. Optimization findings of MOORA

The final ranking of alternatives obtained using the MOORA method is presented in Table 5. The results indicate that Run 13 achieves the highest assessment value (y i = 0.016) and therefore represents the optimal machining condition among the experimental runs. The corresponding process parameters are I p = 4 A, T on = 100 µs, and A p = 10 g/L.

Table 5

MOORA for MRR, TWR, and R a.

RunMRRTWR R a y i
ValueRank
14.30530.82482.34−0.0256
23.51540.46421.820.0083
33.8630.80381.98−0.02710
43.14630.70343.42−0.07715
52.74480.45031.96−0.0195
63.85450.94552.77−0.06714
72.89240.63312.36−0.04812
83.63710.56333.45−0.04411
94.07200.82973.28−0.05913
102.72590.31191.320.0152
113.19130.57592.18−0.0267
123.15900.57192.19−0.0278
13 3.4707 0.3451 2.02 0.016 1
143.29550.43452.64−0.0174
153.16760.57912.17−0.0279

3.5.3. Comparing optimization findings

A comparative analysis between the DA method and the MOORA method was carried out to evaluate their effectiveness in optimizing the PMEDM process. As presented in Table 6, the two optimization techniques produced different optimal machining conditions due to their distinct aggregation principles. The DA method identified the optimal parameter combination as I p = 8 A, T on = 50 µs, and A p = 10 g/L. Under these conditions, the predicted responses were TWR = 0.7159 mg/min, MRR = 4.1170 mg/min, and R a = 1.87 µm. These results indicate that the DA method achieves relatively high removal and tool wear, while SR is improved. In contrast, the MOORA method selected I p = 4 A, T on = 100 µs, and A p = 10 g/L as the optimal setting. The corresponding response values were TWR = 0.3451 mg/min, MRR = 3.4707 mg/min, and R a = 2.02 µm. Compared with the DA method, this configuration resulted in higher SR, along with a reduction in MRR and TWR. A quantitative comparison shows that, relative to MOORA, the DA solution reduced R a by 7.43%, while increasing MRR by 18.62% and TWR by 107.45%. Conversely, MOORA led to a 51.79% reduction in TWR and a 15.7% decrease in MRR, together with an 8.02% increase in R a compared to DA. Overall, the DA method prioritizes higher productivity and slightly improved surface quality, whereas MOORA emphasizes minimizing tool wear at the expense of machining rate. Therefore, the selection of the optimal strategy depends on whether productivity or tool life is considered the primary objective.

Table 6

Comparison of optimal results.

Optimization methodInput parametersOutput responses
I p (A) T on (µs) A p (g/L)TWR (mg/min)MRR (mg/min) R a (µm)
DA850100.71594.11701.87
MOORA4100100.34513.47072.02
Compare DA with MOORA↑ 107.45%↑ 18.62%↓ 7.43%
Compare MOORA with DA↓ 51.79%↓ 15.7%↑ 8.02%

The different optimal solutions obtained from DA and MOORA can be attributed not only to the different aggregation procedures employed by the two methods but also to their fundamentally different optimization frameworks. In the present study, the DA method evaluates the desirability of the machining responses based on the predictive regression models developed for MRR, TWR, and R a. Each response is transformed into an individual desirability function, and these individual desirabilities are then aggregated into an overall desirability index through a weighted geometric mean. Therefore, DA enables the optimization to be performed continuously within the investigated process parameter space rather than being restricted to the experimentally tested combinations. The optimal solution is consequently determined as the parameter combination that provides the best overall compromise among maximizing MRR and minimizing TWR and R a, according to the assigned response weights.

In contrast, MOORA is primarily a multi-criteria ranking method applied to a finite set of alternatives. In this study, the 15 experimental runs constitute the alternatives, while MRR, TWR, and R a are treated as the decision attributes. After normalization and weighting of these attributes using the CRITIC method, an assessment value is calculated for each experimental alternative, and the alternatives are ranked according to their overall performance. Thus, MOORA selects the best-performing alternative from the available experimental runs rather than searching continuously for an optimum within the entire experimental design space.

The difference is particularly evident in the trade-off between productivity and tool wear. The DA solution favors a substantially higher MRR and slightly lower R a, but this is accompanied by a markedly higher TWR. Specifically, compared with MOORA, DA increases MRR by 18.62% and reduces R a by 7.43%, while TWR increases by 107.45%. Conversely, MOORA reduces TWR by 51.79% relative to DA, but MRR decreases by 15.70% and R a increases by 8.02%. These differences should therefore not be interpreted as an inconsistency between the two optimization methods. Rather, they demonstrate that the two approaches identify different forms of compromise because DA performs multi-response optimization through desirability functions based on the regression models, whereas MOORA ranks discrete experimentally observed alternatives.

From a practical perspective, the DA solution is more appropriate when the objective is to identify a process condition that provides the best overall compromise within the investigated parameter domain and when the predictive response models are considered reliable. The MOORA solution is particularly useful when the selection must be made directly among experimentally tested parameter combinations and when minimizing tool wear is given greater practical importance through the resulting multi-criteria ranking. Therefore, the choice between DA and MOORA should depend on the intended decision-making framework rather than on considering one method as universally superior to the other.

3.5.4. The experimental validation of the optimal parameters determined by the DA and MOORA methods

The experimental results obtained at the optimum machining conditions are summarized in Table 7. A comparison between the predicted responses and their corresponding experimental measurements reveals only minor discrepancies. Among the investigated responses, the largest deviation, namely 3.16%, is observed for TWR when the MOORA approach is employed, while the smallest difference of 1.05% is associated with TWR determined using the DA technique. The limited deviations between the calculated and measured results confirm the satisfactory accuracy of the developed predictive models and the effectiveness of the applied optimization methods.

Table 7

Validation experiments of the optimal results.

MethodMachining responsesOptimal parametersPre. valuesExp. valuesError (%)
DAMRR, mg/min I p = 8 A, T on = 50 µs, C p = 10 g/L4.11704.2112 ± 0.04882.28
TWR, mg/min0.71590.7234 ± 0.00771.05
R a, μm1.871.84 ± 0.01841.6
MOORAMRR, mg/min I p = 4 A, T on = 100 µs, C p = 10 g/L3.47073.5604 ± 0.03702.58
TWR, mg/min0.34510.3342 ± 0.00373.16
R a, μm2.021.96 ± 0.02002.97

Error = Abs (Pred. values − Exp. values)/Pred. values × 100%.

As stated, the optimization work was assessed. However, additional analysis is necessary to gain a deeper understanding of surface attributes from ideal settings. This helps professionals select the optimal machining parameters.

The surface defects at the optimum modes of these two algorithms were investigated (Figure 7). Figure 6a and b represents the surface morphology at the optimum parameters of the DA and MOORA algorithms, respectively. It is clear that the defects of surfaces like the droplet number (the circle marked red color), the debris globule number (the circle marked yellow color), the micro-crack number (the track marked green color), and the void number (the circle marked blue color) of Figure 6a are lesser than those of Figure 6b. Evidently, the value of I p obtained by the DA is greater than that of the MOORA, while the value of T on obtained by the DA is smaller than that of the MOORA, and A p of both the MOORA and DA methods is equal. Therefore, an increase in T on could raise the presence of surface defects [23,24]. This is all associated with the powder participation in the discharge operation. Since the discharge channel is dominated by powder particles, which results in stratification in the spark discharge operation, modifications in the eroded material, generated redundancy stress on the surface, and attributes of the solvent such as viscosity, electrical conductivity, and heat transfer are altered [25].

Figure 7

Surface flaws in optimizing parameters: (a) DA and (b) MOORA.

An examination of the surface chemical composition reveals a clear difference between the elemental profiles produced under the optimal conditions identified by DA and MOORA, as illustrated in Figure 8. Specifically, higher proportions of C, O, Mn, Co, Mo, and W are detected for the DA-derived condition, whereas Si, V, Cr, Fe, and Cu exhibit greater concentrations when the MOORA-based setting is employed. Such variations can be attributed to the different combinations of optimal process parameters delivered by the two optimization approaches, which alter the characteristics of discharge events and consequently influence the associated physical and chemical phenomena. Furthermore, the spatial distributions of the detected elements under the two optimal conditions are presented in Figures 9 and 10. Compared with the MOORA condition (Figure 10), the elemental constituents generated using the DA parameters (Figure 9) exhibit a more homogeneous distribution across the machined surface. This discrepancy may originate from the distinct process-parameter combinations, which promote differences in discharge-channel development and thereby modify the mechanisms governing material transfer, deposition, and surface modification [26].

Figure 8

Compositional chemistry and element content on surfaces at optimum parameters: (a) DA; (b) MOORA.

Figure 9

Distribution of chemical elements at optimal parameters derived from the DA method.

Figure 10

Distribution of chemical elements at optimal parameters derived from the MOORA method.

Regarding the recast layer, the specimen produced under the DA-optimized condition exhibits a lower layer thickness than the one obtained using MOORA, as illustrated in Figure 11. Moreover, the deposited layer generated under the DA condition appears to be more homogeneous and consistent across the machined surface. The discrepancies observed between the two optimization strategies can be attributed primarily to differences in the selected electrical discharge parameters. Such variations modify the decomposition and expansion behavior of gas bubbles generated during individual discharge events, which subsequently influences the interaction between the suspended powder particles and the plasma channel during the following discharges [27,28]. The presence of an appropriate powder concentration promotes a more stable and spatially distributed discharge while simultaneously enlarging the effective discharge region [29,30]. Furthermore, the EDM oil facilitates the removal of molten and resolidified debris from the machining gap by maintaining favorable dielectric-flow conditions. The combined effects of these phenomena ultimately lead to differences in the thickness and morphological uniformity of the recast layers produced under the two optimized conditions.

Figure 11

Thickness of the recast layer: (a) DA and (b) MOORA.

4. Conclusions

In this investigation, SKD11 steel was processed by EDM using a tungsten powder alloy. The main findings are summed up as follows:

  • All output qualities rise with an increase in I p or T on. When A p is increased, MRR increases, TWR decreases, and R a either decreases or increases. In particular, I p has the greatest influence on MRR, contributing 59.48%, followed by A p (20.96%) and T on (5.32%). I p has the largest impact on TWR, accounting for 87.48% of the total, followed by A p at 7.22% and T on at 2.55%. For R a, T on has the biggest impact on R a, accounting for 66.82% of the contribution, followed by I p and A p, which accounts for 13.99% and 1.84%, respectively.

  • The developed predictive models exhibit high coefficients of determination, with R² values of 0.9961 for TWR, 0.9932 for MRR, and 0.9987 for R a. Consequently, the proposed models can be reliably used to estimate the corresponding output attributes.

  • MOORA and DA were utilized to determine the optimal solution under multiple performance criteria. The DA approach demonstrated superior performance in enhancing MRR and SR compared with MOORA, achieving an 18.62% increase in MRR and a 7.43% reduction in R a. In contrast, MOORA outperformed DA in minimizing TWR, yielding a reduction of 51.79%.

  • The optimal parameter sets obtained from the DA and MOORA methods were employed to evaluate surface characteristics. As a result, the DA-based conditions produced a thinner recast layer and fewer surface defects compared with those derived from MOORA. The higher proportions of C, O, Mn, Co, Mo, and W were detected for the DA-derived condition, whereas Si, V, Cr, Fe, and Cu exhibited greater concentrations when the MOORA-based setting was employed. For the distribution of compositional chemistry, the compositional chemistry obtained from the optimum parameters of DA resulted in a more uniform distribution than that of MOORA.

  • Both DA and MOORA address the multi-objective optimization problem and yield optimal parameter combinations. Nevertheless, the selection of a specific method depends on whether priority is given to surface integrity or machining performance criteria.

  • The results of this investigation enhance insight into the strengths of the DA and MOORA techniques, along with the machining behavior of SKD11 steel in tungsten powder–assisted EDM. These insights are valuable for both industrial applications and academic research.

Funding information

Authors state no funding involved.

Author contributions

Manh-Tung Do: Investigation, data curation, formal analysis, visualization, and writing - original draft. Van-Tao Le: Conceptualization, methodology, supervision, project administration, and writing - review and editing. Long Hoang, Truong-Giang Nguyen, Ngoc-Quy Nguyen, and Ba-Bao Nguyen: Investigation, resources, validation, and writing – review and editing. All authors read and approved the final manuscript.

Conflict of interest statement

Authors state no conflict of interest.

Data availability statement

The data supporting the findings of this study are available from the corresponding author upon reasonable request.

DOI: https://doi.org/10.2478/msp-2026-0018 | Journal eISSN: 2083-134X (formerly 2083-124X) | Journal ISSN: 2083-1331
Language: English
Page range: 106 - 125
Submitted on: May 15, 2026
Accepted on: Sep 13, 2026
Published on: Oct 26, 2026
Published by: Wroclaw University of Science and Technology
In partnership with: Paradigm Publishing Services

© 2026 Manh-Tung Do, Van-Tao Le, Long Hoang, Truong-Giang Nguyen, Ngoc-Quy Nguyen, Ba-Bao Nguyen, published by Wroclaw University of Science and Technology
This work is licensed under the Creative Commons Attribution-NonCommercial-NoDerivatives 4.0 License.