Table 1:

The mechanical properties of the Profiber CW300

BrandWeight [g/m2]Design thickness [mm]Tensile strength [MPa]Tensile E-modulus [GPa]Elongation at break [%]
DCP PROFIBER CW3003000.16648002301.7
Figure 1:

Geometry of the non-prismatic test specimen of columns

Figure 2:

Fabrication of the specimens

Figure 3:

Performing specimens test to axial loading

Figure 4:

Instrumentation arrangement of the lateral loading

Figure 5:

Layout of the testing rig

Figure 6:

Rehabilitation using ferrocement jacketing

Figure 7:

Rehabilitation using steel jacketing

Table 2:

The performance levels according to ACI-374-2R-13 in terms of the drift ratio

Drift statusPerformance level
OP operationalIO immediate occupancyLS life safetyCP collapse prevention
Transient drift (temporary)<<1%≤1%≤2%≤4%
Permanent drift (residual)<<1%<1%≤1%≤4%
Figure 8:

Cyclic loading history

Table 3:

Protocol imposed on specimens (FJLA20 & SJLA20) in terms of performance level

Cycle No.AmplitudeDisplacement [mm]Drift ratio [%]Transient performance level
10.5Δy3.70.27IO
2Δy7.40.54IO
32Δy14.81.09LS
43Δy22.21.64LS
54Δy29.62.19CP
65Δy37.02.74CP
76Δy44.43.28CP
Table 4:

Protocol imposed on specimens (FJLA40 & SJLA40) in terms of performance level

Cycle No.AmplitudeDisplacement [mm]Drift ratio [%]Transient performance level
10.5Δy2.90.21IO
2Δy5.70.43IO
32Δy11.40.84IO
43Δy17.11.26LS
54Δy22.81.68LS
65Δy28.52.11CP
76Δy34.22.53CP
Table 5:

Axial load test results for non-prismatic RC columns

DescriptionNPRIS-0NPRIS-1Average
Max. load [kN]854.4955.8905.1
Axial displ. at max load [mm]3.0363.863.448
Strain in the rebar at max load−0.0027−0.0028−0.00275
Strain in the stirrup at max load0.00140.00150.00145
Axial stiffness [kN/m]312,100349,649330,874
Toughness [J]1047.515771312
Figure 9:

Shear failure mode in non-prismatic specimens

Figure 10:

Axial load – deflection curves for NPRIS-0 & NPRIS-1

Table 6:

Pushover test results (yield and ductility parameters)

SpecimenAxial loadΔy [mm]Py [kN]Δu [mm]μd = Δu/Δy
LA2020% (181 kN)7.3517.262.68.52
LA4040% (362 kN)5.7032.027.434.80
Figure 11:

Pushover behaviour under 20% & 40% axial load

Figure 12:

Cracking pattern in the specimens LA20 & LA40 after pushover test

Table 7:

Dissipated energy prior to the rehabilitation (kN·mm)

SpecimenCycle 1 [0.5Δy]Cycle 2 (0.5Δy)Cycle 3 (Δy)Cycle 4 (Δy)Total
FJLA2062.1245.66145.28108.51361.57
SJLA2038.7230.88131.53100.65301.78
FJLA4037.1423.43127.2882.71270.56
SJLA4035.4325.46131.3863.67255.94
Figure 13:

Displacement protocol imposed on test specimens before rehabilitation

Figure 14:

Cyclic behaviour of FJLA20 specimen under 181kN axial load

Figure 15:

Cyclic behaviour of SJLA20 specimen under 181kN axial load

Figure 16:

Cyclic behaviour of FJLA40 specimen under 362kN axial load

Figure 17:

Cyclic behaviour of SJLA40 specimen under 362kN axial load

Figure 18:

Pre rehabilitation dissipated energy

Table 8:

Cumulative dissipated energy after rehabilitation (kN.mm)

Axial load ratioFerrocement jacketSteel-plate jacketDifference (ferrocement vs. steel)
20%8,927.88,188.2+9.0%
40%8,084.68,034.8+0.6%
Table 9:

Residual deformation and resulting performance-level classification

SpecimenPermanent deformation at final cycle [mm]Performance level
FJLA2021.14Collapse prevention (CP)
FJLA4019.88Collapse prevention (CP)
SJLA2010.41Life safety (LS)
SJLA4012.79Collapse prevention CP (close to Life safety boundary)
Figure 19:

Hysteresis loops for FJLA20 after the rehabilitation

Figure 20:

Hysteresis loops for SJLA20 after the rehabilitation

Figure 21:

Hysteresis loops for FJLA40 after the rehabilitation

Figure 22:

Hysteresis loops for SJLA40 after the rehabilitation

Figure 23:

Comparison among pushover, damaged induction, and post rehabilitation response

DOI: https://doi.org/10.2478/cee-2027-0038 | Journal eISSN: 2199-6512 (formerly 1336-5835) | Journal ISSN: 1336-5835
Language: English
Submitted on: Sep 2, 2026
Accepted on: Sep 24, 2026
Published on: Nov 20, 2026
Published by: University of Žilina
In partnership with: Paradigm Publishing Services
Publication frequency: 4 issues per year

© 2026 Romaih O. Mostafa, Sofyan Y. Ahmed, Jasim A. Abdullah, published by University of Žilina
This work is licensed under the Creative Commons Attribution 4.0 License.