Skip to main content
Have a personal or library account? Click to login
Thermal conductivity of polyurethane insulation boards subjected to temporary compression Cover

Thermal conductivity of polyurethane insulation boards subjected to temporary compression

Open Access
|Jul 2026

Figures & Tables

Fig. 1.

Insulation under the foundation slab in the model (Izodom 2000 Polska Sp. z o.o., Zduńska Wola) single-family house (photo: Zbigniew Respondek)

Fig. 2.

General view: a) Heat Flow Meter Netzsch HFM 446, b) sample PIR, c) sample PUR (own photos)

Fig. 3.

Example graph generated by the device (own research)

Fig. 4.

XPS sample seasoning under load (own photo)

Measurement results of the XPS sample thickness (own research)

DescriptionSample thickness
d0(in) [cm]d0(fi) [cm]Diff [%]d30(in) [cm]d30(fi) [cm]Diff [%]
Test 110.149310.1308−0.1810.143010.1258−0.17
Test 210.146910.1267−0.2010.142710.1216−0.21
Test 310.145310.1312−0.1410.143710.1267−0.17
Average of Diff−0.17 %−0.18 %

Measurement results of the λ-value for the PIR sample (own research)

DescriptionThermal conductivity
λ0 [W/(m·K)]λ30 [W/(m·K)]
Test 10.020800.02100
Test 20.020730.02115
Test 30.021040.02111
Average of measurements0.020860.02109
Declared by the manufacturer0.22

Measurement results of the λ-value for the PUR sample (own research)

DescriptionThermal conductivity
λ0 [W/(m·K)]λ30 [W/(m·K)]
Test 10.021140.02130
Test 20.020730.02118
Test 30.021090.02135
Average of measurements0.021090.02128
Declared by the manufacturer0.21

Measurement results of the PIR sample thickness (own research)

DescriptionSample thickness
d0(in) [cm]d0(fi) [cm]Diff [%]d30(in) [cm]d30(fi) [cm]Diff [%]
Test 110.053010.0204−0.3210.064210.0460−0.18
Test 210.060210.0358−0.2410.069110.0565−0.13
Test 310.064410.0389−0.2510.067710.0463−0.21
Average of Diff−0.27 %−0.17 %

Measurement results of the λ-value for the XPS sample (own research)

DescriptionThermal conductivity
λ0 [W/(m·K)]λ30 [W/(m·K)]
Test 10.030220.03122
Test 20.030670.03112
Test 30.030520.03125
Average of measurements0.030470.03120
Declared by the manufacturer0.35

Measurement results of the PUR sample thickness (own research)

DescriptionSample thickness
d0(in) [cm]d0(fi) [cm]Diff [%]d30(in) [cm]d30(fi) [cm]Diff [%]
Test 110.171010.1633−0.0810.164510.1533–0.11
Test 210.169510.1516−0.1810.165810.1543–0.11
Test 310.168010.1594−0.0810.166410.1553–0.11
Average of Diff−0.11 %−0.11 %
DOI: https://doi.org/10.17512/bozpe.2026.15.07 | Journal eISSN: 2544-963X | Journal ISSN: 2299-8535
Language: English
Published on: Jul 13, 2026
In partnership with: Paradigm Publishing Services
Publication frequency: 1 issue per year

© 2026 Zbigniew Respondek, Kacper Woźny, published by Technical University in Czestochowa
This work is licensed under the Creative Commons Attribution-NonCommercial-ShareAlike 4.0 License.

AHEAD OF PRINT